Jump to content

Specific Process Knowledge/Thin Film deposition/ALD/TiO2 deposition using ALD: Difference between revisions

From LabAdviser
Eves (talk | contribs)
No edit summary
Pevo (talk | contribs)
No edit summary
Line 36: Line 36:
|-
|-
|}
|}


In the graphs below the TiO<sub>2</sub> thickness as function of the number of cycles for deposition temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C can be seen. From the equations the number of cycles required for a certain thickess can be calculated.  
In the graphs below the TiO<sub>2</sub> thickness as function of the number of cycles for deposition temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C can be seen. From the equations the number of cycles required for a certain thickess can be calculated.  
Line 45: Line 43:
image:ALD_TiO2_grow_rate_250C.jpg| Temperature 250 <sup>o</sup>C.
image:ALD_TiO2_grow_rate_250C.jpg| Temperature 250 <sup>o</sup>C.
image:ALD_TiO2_grow_rate_350C.jpg| Temperature 350 <sup>o</sup>C.
image:ALD_TiO2_grow_rate_350C.jpg| Temperature 350 <sup>o</sup>C.
</gallery>
Some some SEM images of TiO<sub>2</sub> deposited on a silicon surface at different temperatures between 150 <sup>o</sup>C and 120 <sup>o</sup>C are shown below:
<gallery caption="Titanium dioxide thickness as function of number of cycles" widths="200px" heights="200px" perrow="5">
image:TiO2 150C 1200 cycles Si_HF_treated.jpg| Temperature 150 <sup>o</sup>C.
image:TiO2 150C 1200 cycles Si_untreated.jpg| Temperature 250 <sup>o</sup>C.
image:TiO2 250C 750cycles_Si_untreated.jpg| Temperature 350 <sup>o</sup>C.
image:TiO2 1000 cycles 300C Si_HF.jpg| Temperature 350 <sup>o</sup>C.
image:TiO2 1000 cycles 300C Si_un.jpg| Temperature 350 <sup>o</sup>C.
image:TiO2 350C 1250 cycles Si_HF_treated.jpg| Temperature 350 <sup>o</sup>C.
</gallery>
</gallery>



Revision as of 15:20, 2 July 2015

THIS PAGE IS UNDER CONSTRUCTION

Feedback to this page: click here

The ALD window for titanium dioxide (TiO2) ranges from 120 oC to 350 oC.

A low temperatures between 120 oC and 150 oC an anatase TiO2 layer is grown in the ALD, and at higher temperatures between 300 oC and 350 oC an amorphous TiO2 layer is grown. At temperatures between 150 oC and 300 oC the TiO2 layer will be a mixture of both anatase and amorphous TiO2.

For Si wafers, anatase TiO2 is best grown on wafers without native oxide (removed using BHF), and amorphous TiO2 is best grown on wafers with native oxide.

XPS measurements shows that at temperaturs below 120 oC the TiO2 layer will be contaminated with about 1-3 % chlorine molecules from the TiCl4 precursor. This can be seen as small white dots in SEM images of the anatase TiO2 layers.


Recipe: TiO2

Temperature: 120 oC - 350 oC

TiCl4 H2O
Nitrogen flow 150 sccm 200 sccm
Pulse time 0.1 s 0.1 s
Purge time 3.0 s 4.0 s

In the graphs below the TiO2 thickness as function of the number of cycles for deposition temperatures between 150 oC and 350 oC can be seen. From the equations the number of cycles required for a certain thickess can be calculated.

Some some SEM images of TiO2 deposited on a silicon surface at different temperatures between 150 oC and 120 oC are shown below:

Below some SEM images of anatase TiO2 deposited at 120 oC on Si trenches are shown. The width of the trenches is 200 nm, and the depth is 4 µm, i.e. the aspect ratio is 1:20. The number of cycles is 500, and this results in a TiO2 layer of about 25 nm. From the SEM images it is seen that the TiO2 layer covers the trenches very well.

Below some SEM images of amorphous TiO2 deposited at 300 oC on Si trenches are shown. The width of the trenches is 200 nm, and the depth is 4 µm, i.e. the aspect ratio is 1:20. The number of cycles is 500, and this results in a TiO2 layer of about 26 nm. From the SEM images it is seen that the TiO2 layer covers the trenches very well.

Evgeniy Shkondin, DTU Danchip, 2014.