Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/Sinan33-2: Difference between revisions
Appearance
Created page with "== The Sinano3.3 recipe == {| border="2" cellpadding="2" cellspacing="1" |+ '''Recipe Sinano3.3''' |- ! rowspan="6" align="center"| Recipe | Gas | BCl<sub>3</sub> 5 sccm, HB..." |
|||
| Line 1: | Line 1: | ||
== The Sinano3.3 recipe == | == The Sinano3.3 recipe == | ||
<!-- revised 1/6-2015 by jmli --> | |||
{| border="2" cellpadding="2" cellspacing="1" | {| border="2" cellpadding="2" cellspacing="1" | ||
|+ '''Recipe Sinano3.3''' | |+ '''Recipe Sinano3.3''' | ||
Revision as of 14:12, 1 June 2015
The Sinano3.3 recipe
| Recipe | Gas | BCl3 5 sccm, HBR 15 sccm |
|---|---|---|
| Pressure | 2 mTorr, Strike 3 secs @ 5 mTorr | |
| Power | 900 W CP, 75 W PP | |
| Temperature | 20 degs | |
| Hardware | 100 mm Spacers | |
| Time | 300 secs | |
| Conditions | Run ID | 444 |
| Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | |
| Mask | 348 nm zep etched down to 53 nm |
- The results of the Sinano3.3 recipe
-
The 30 nm trenches
-
The 60 nm trenches
-
The 90 nm trenches
-
The 120 nm trenches
-
The 150 nm trenches
| Nominal trench line width | ' | ' | 30 | 60 | 90 | 120 | 150 | Average | Std. dev. |
| Etch rate | nm/min | 59 | 82 | 114 | 120 | 129 | 101 | 29 | |
| Sidewall angle | degs | 85 | 83 | 83 | 82 | 81 | 83 | 2 | |
| CD loss | nm/edge | -1 | 0 | -5 | -7 | -13 | -5 | 5 | |
| CD loss foot | nm/edge | -1 | 0 | -5 | -7 | 18 | 1 | 10 | |
| Bowing | 18 | 27 | 36 | 38 | 23 | 28 | 9 | ||
| Bottom curvature | -41 | -27 | -16 | -30 | -9 | -24 | 12 | ||
| Zep etch rate | 59 |