'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/ICP_Metal_Etcher/Barc_Etch click here]''' | '''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/Barc_Etch click here]''' | ||
==Barc Etch== | ==Barc Etch== | ||
Revision as of 13:25, 19 May 2015
Feedback to this page: click here
Barc Etch
Etching barc with a dedicated recipe for barc etching is a good idea if you are on the limit of having enough DUV resist mask to reach etch depth you need.Here is an example of a barc etch I have started testing.
| Parameter | Barc etch with CF4 |
|---|---|
| Coil power | 800W |
| Platen power | 100W |
| Pressure | 3 mTorr |
| Flow rate CF4 | 4 sccm |
| Flow rate H2 | 20sccm |
| Parameter | Results |
|---|---|
| Etch rate in barc | 52nm in 30s |
| Etch rate in KRF resist | 27 nm in 30s |
| Selectivity KRF:Barc | 1:2 |
| Etch 65nm barc | Use 40-45s |