Negative replicas of micro- or nanostructures can be obtained by casting with PDMS. This can facilitate the characterization of the three dimensional shape, the texture, or the roughness of a given sample. It may circumvent the inabilities of probes (AFM tip, stylus) to approach a surface of e.g. a deep and narrow cavity. It may also circumvent limitations of the optical profiler regarding the maximum detectable slope or the sensitivity of the CCD when measuring strongly tapered or deep cavities. PDMS is a common material in microfabrication and has unique properties that allow replicating features in the single nanometer range [1]. | Negative replicas of micro- or nanostructures can be obtained by casting with PDMS. This can facilitate the characterization of the three dimensional shape, the texture, or the roughness of a given sample. It may circumvent the inabilities of probes (AFM tip, stylus) to approach a surface of e.g. a deep and narrow cavity. It may also circumvent limitations of the optical profiler regarding the maximum detectable slope or the sensitivity of the CCD when measuring strongly tapered or deep cavities. PDMS is a common material in microfabrication and has unique properties that allow replicating features in the single nanometer range [1]. | ||
* | * A simplified list of necessary steps is given below. Please follow the safety and working rules of the individual lab the work is done in and consider the safety instructions given in [2]. | ||
* Please be aware that it is not allowed to work with PDMS in its uncured state inside the cleanroom. The list of approved chemicals inside the cleanroom still holds. | |||
* Details on Danchip’s experience with PDMS as a casting material may be found in [3] (please cite!). A detailed description for PDMS casting can be found in [2] and practical information is given in [4]. | |||
* The most important steps for obtaining high quality casts are the thorough mixing of the two components of the PDMS Kit (Sylgard 184, Dow Corning) and the sufficient outgassing of the polymer prior and after pouring the polymer into the mould. The house vacuum may be too weak. For special demands, try to get hold of a separate pump like a HiCube Classic from Pfeiffer Vacuum [4] (there is one around at DTU Photonics or Danchip). | |||
* The application of an anti-stiction coating, like FDTS, is necessary. It may be applied inside the cleanroom by the MVD. Contact the respective person. | |||
* The mold may be reused upon casting without deterioration (try!) | |||
==A simplified list of necessary steps== | ==A simplified list of necessary steps== | ||
Revision as of 18:43, 12 May 2015
Replica Molding for Sample Inspection
Negative replicas of micro- or nanostructures can be obtained by casting with PDMS. This can facilitate the characterization of the three dimensional shape, the texture, or the roughness of a given sample. It may circumvent the inabilities of probes (AFM tip, stylus) to approach a surface of e.g. a deep and narrow cavity. It may also circumvent limitations of the optical profiler regarding the maximum detectable slope or the sensitivity of the CCD when measuring strongly tapered or deep cavities. PDMS is a common material in microfabrication and has unique properties that allow replicating features in the single nanometer range [1].
- A simplified list of necessary steps is given below. Please follow the safety and working rules of the individual lab the work is done in and consider the safety instructions given in [2].
- Please be aware that it is not allowed to work with PDMS in its uncured state inside the cleanroom. The list of approved chemicals inside the cleanroom still holds.
- Details on Danchip’s experience with PDMS as a casting material may be found in [3] (please cite!). A detailed description for PDMS casting can be found in [2] and practical information is given in [4].
- The most important steps for obtaining high quality casts are the thorough mixing of the two components of the PDMS Kit (Sylgard 184, Dow Corning) and the sufficient outgassing of the polymer prior and after pouring the polymer into the mould. The house vacuum may be too weak. For special demands, try to get hold of a separate pump like a HiCube Classic from Pfeiffer Vacuum [4] (there is one around at DTU Photonics or Danchip).
- The application of an anti-stiction coating, like FDTS, is necessary. It may be applied inside the cleanroom by the MVD. Contact the respective person.
- The mold may be reused upon casting without deterioration (try!)
A simplified list of necessary steps
| Step | Task | Aim | Methods |
|---|---|---|---|
| 1 | Sample preparation | A mold containing the sample that is sufficiently sealed to allow holding the viscous polymer. | Some parts from the mechanical workshop, etc. Do not forget poper cleaning. |
| 2 | Anti-stiction coating | A sample to which PDMS does not adhere upon casting. | E.g. MVD -> FDTS layer (comply to cleanroom and machine rules) |
| 3 | Sample preparation | A mold containing the sample that is sufficiently sealed to allow holding the viscous polymer. | Some parts from the mechanical workshop, etc. Do not forget poper cleaning. |
| 4 | Sample preparation | A mold containing the sample that is sufficiently sealed to allow holding the viscous polymer. | Some parts from the mechanical workshop, etc. Do not forget poper cleaning. |
| 5 | Sample preparation | A mold containing the sample that is sufficiently sealed to allow holding the viscous polymer. | Some parts from the mechanical workshop, etc. Do not forget poper cleaning. |
| 6 | Sample preparation | A mold containing the sample that is sufficiently sealed to allow holding the viscous polymer. | Some parts from the mechanical workshop, etc. Do not forget poper cleaning. |
| 7 | Sample preparation | A mold containing the sample that is sufficiently sealed to allow holding the viscous polymer. | Some parts from the mechanical workshop, etc. Do not forget poper cleaning. |
| 8 | Sample preparation | A mold containing the sample that is sufficiently sealed to allow holding the viscous polymer. | Some parts from the mechanical workshop, etc. Do not forget poper cleaning. |
| 9 | Sample preparation | A mold containing the sample that is sufficiently sealed to allow holding the viscous polymer. | Some parts from the mechanical workshop, etc. Do not forget poper cleaning. |