Etching of Gold

Etching of Gold is done wet at Danchip making your own set up in a beaker in the fumehood. We have two different solutions:
- Iodine etch: KI:I:HO - 100g:25g:500ml - standard at Danchip. Can be used with AZ resist as mask.
- Aqua Regia (Kongevand): HNO:HCl - 1:3 - A very strong acid witch will etch most metals and are therefore used when you wish to remove all the gold from your wafer. you have to be very carefull when you work with Aqua Regia (Kongevand) It can generate nitrous gases witch are very toxic!!
Comparing the two solutions
| Iodine based gold etch | Aqua Regia (Kongevand) | |
|---|---|---|
| General description |
Etch of pure Gold with or without photoresist mask. |
Etch of pure Gold (as stripper). |
| Chemical solution | KJ:J:HO (100g:25g:500ml) | HCl:HNO (3:1) |
| Process temperature | 20 oC | 20 oC |
| Possible masking materials |
Photoresist (1.5 µm AZ5214E) |
Unmasked - used as a stripper |
| Etch rate |
~100 nm/min |
~(??) nm/min - fast etch |
| Batch size |
1-25 wafers at a time |
1-25 wafer at a time |
| Size of substrate |
2-6" wafers |