!Chemical solution
|HNO<math>_3</math>:H<math>_2</math>O:cerisulphate  - 90ml:1200ml:15g
|HNO<math>_3</math>:H<math>_2</math>O:cerisulphate  - 90ml:1200ml:15g
|Commercial chromium etch
|Commercial chromium etch
CE 8002-A
CE 8002-A
|-
|-
|Process temperature
!Process temperature
|Room temperature
|Room temperature


Line 31: Line 31:
|-
|-


|Possible masking materials:
!Possible masking materials:
|
|
Photoresist (1.5 µm AZ5214E)
Photoresist (1.5 µm AZ5214E)
Line 43: Line 43:
~10-20 nm/min
~10-20 nm/min
|-
|-
|Batch size
!Batch size
|
|
1-25 wafers at a time
1-25 wafers at a time
Line 55: Line 55:
4" wafers
4" wafers
|-
|-
|Allowed materials
!Allowed materials
|
|
No restrictions.
No restrictions.

Revision as of 13:54, 31 January 2008

Etching of Chromium

Etching of chromium is done wet at Danchip making your own set up in a beaker in a fume hood - preferably in cleanroom 2 or 4. We have two solution for this:

  1. HNO3:H2O:cerisulphate - 90ml:1200ml:15g - standard at Danchip
  2. Commercial chromium etch

Etch rate are depending on the level of oxidation of the metal.


Chromium etch 1 Chromium etch 2
General description

Etch of chromium

Etch of chromium

Chemical solution HNO3:H2O:cerisulphate - 90ml:1200ml:15g Commercial chromium etch

CE 8002-A

Process temperature Room temperature Room temperature
Possible masking materials:

Photoresist (1.5 µm AZ5214E)

Photoresist (1.5 µm AZ5214E)

Etch rate

~40-100 nm/min

~10-20 nm/min

Batch size

1-25 wafers at a time

1-25 wafer at a time

Size of substrate

4" wafers

4" wafers

Allowed materials

No restrictions. Make a note on the beaker of which materials have been processed.