==Wet Poly Etch==
==Wet PolySi Etch==


[[Image:Wet_PolySi_etch.jpg|300x300px|thumb|Wet PolySilicon Etch (in the middle): positioned in cleanroom 4]]
[[Image:Wet_PolySi_etch.jpg|300x300px|thumb|Wet PolySilicon Etch (in the middle): positioned in cleanroom 4]]


The wet Poly Etch is an isotropic silicon etch. This holds for both a poly-silicon thin-film as well as single-crystalline material such as a Si(100) surface. The Poly Etch process is placed in a dedicated PP-tank in a laminar-flow bench in cleanroom 4.
The wet PolySi Etch is an isotropic silicon etch. This holds for both a poly-silicon thin-film as well as single-crystalline material such as a Si(100) surface. The PolySi Etch process is placed in a dedicated PP-tank in a laminar-flow bench in cleanroom 4.


The Poly Etch is typically used for opening holes in poly-silicon thin-films, using photoresist as an etch mask. Due to its isotropic nature the under-etching (etch-bias) at least amounts to the thickness of the poly-silicon layer. Another example of usage is etching of "circular-shaped" holes in silicon substrates.
The PolySi Etch is typically used for opening holes in poly-silicon thin-films, using photoresist as an etch mask. Due to its isotropic nature the under-etching (etch-bias) at least amounts to the thickness of the poly-silicon layer. Another example of usage is etching of "circular-shaped" holes in silicon substrates.


The Poly Etch is based on the combined oxidation of silicon followed by dissolution of the silicon oxide. The etch solution consists of:
The PolySi Etch is based on the combined oxidation of silicon followed by dissolution of the silicon oxide. The etch solution consists of:


HNO<sub>3</sub> : BHF : H<sub>2</sub>O  - (20 : 1 : 20)
HNO<sub>3</sub> : BHF : H<sub>2</sub>O  - (20 : 1 : 20)