Etching of Gold is done wet at Danchip making your own set up in a beaker in the fumehood. We have two different solutions:
Etching of Gold is done wet at Danchip making your own set up in a beaker in the fumehood. We have two different solutions:


# Iodine etch: KI:I<math>_2</math>:H<math>_2</math>O - 100g:25g:500ml
# Iodine etch: KI:I<math>_2</math>:H<math>_2</math>O - 100g:25g:500ml - standard at Danchip
# Aqua Regia (Kongevand): HNO<math>_3</math>:HCl - 1:3
# Aqua Regia (Kongevand): HNO<math>_3</math>:HCl - 1:3



Revision as of 10:58, 31 January 2008

Etching of Gold

Etching of Gold is done wet at Danchip making your own set up in a beaker in the fumehood. We have two different solutions:

  1. Iodine etch: KI:I2:H2O - 100g:25g:500ml - standard at Danchip
  2. Aqua Regia (Kongevand): HNO3:HCl - 1:3


Comparing the two solutions

Iodine based gold etch Aqua Regia (Kongevand)
General description

Etch of pure Gold

Etch of pure Gold

Chemical solution KJ:J2:H2O (100g:25g:500ml) HCl:HNO3 (3:1)
Process temperature 20 oC 20 oC
Possible masking materials:

Photoresist (1.5 µm AZ5214E)

Unmasked - used as a stripper

Etch rate

~100 nm/min

~(??) nm/min

Batch size

1-25 wafers at a time

1-25 wafer at a time

Size of substrate

2-6" wafers

2-6" wafers