Jump to content

Specific Process Knowledge/Thermal Process/Oxidation/Wet oxidation C1 furnace: Difference between revisions

From LabAdviser
Paphol (talk | contribs)
Paphol (talk | contribs)
Line 41: Line 41:
====Results (1)====
====Results (1)====


The figure 1 shows that the silicon dioxide thickness over the boat is affected the most by process time, temperature and steamer flow rate respectively. When the process time, temperature and steamer flow rate increase, the silicon dioxide thickness also increases. Since the steamer flow has the least an effect to the silicon dioxide thickness, so the flow rate has been fixed at 10 liters per minutes in the furnace recipe.
The figure 1 shows that the silicon dioxide thickness over the boat is affected the most by growth time, temperature and steamer flow rate respectively. When the growth time, temperature and steamer flow rate increase, the silicon dioxide thickness also increases. Since the steamer flow has the least an effect to the silicon dioxide thickness, so the flow rate has been fixed at 10 liters per minutes in the furnace recipe.




Line 53: Line 53:




The percent of film non-uniformity over the boat most likely depends on the silicon dioxide thickness. The thicker silicon dioxide gives better film uniformity. The figure 1 shows that the percent of film non-uniformity over the boat decreases, when the process time, steamer flow rate and the temperature increase.
The percent of film non-uniformity over the boat most likely depends on the silicon dioxide thickness. The thicker silicon dioxide gives better film uniformity. The figure 1 shows that the percent of film non-uniformity over the boat decreases, when the growth time, steamer flow rate and the temperature increase.




'''
'''
[[image:Steamer_process_develop_fig2.png|527 × 324 px|middle|The average silicon dioxide thickness and the percent of film non-uniformity over the wafer variation with process time, steamer flow rate and temperature.]]
[[image:Steamer_process_develop_fig2.png|527 × 324 px|middle|The average silicon dioxide thickness and the percent of film non-uniformity over the wafer variation with growth time, steamer flow rate and temperature.]]


'''
'''


'''Figure 2.''' The average silicon dioxide thickness and the percent of film non-uniformity over the wafer variation with process time, steamer flow rate and temperature.
'''Figure 2.''' The average silicon dioxide thickness and the percent of film non-uniformity over the wafer variation with growth time, steamer flow rate and temperature.
'''
'''




The effect of the steamer flow rate, process time and temperature to the silicon dioxide thickness and to the percent of film non-uniformity over the wafer is quite similar with over the boat. But the percent of film non-uniformity over the boat is lower than over the boat, and the steamer flow has almost no an effect on the film uniformity.
The effect of the steamer flow rate, growth time and temperature to the silicon dioxide thickness and to the percent of film non-uniformity over the wafer is quite similar with over the boat. But the percent of film non-uniformity over the boat is lower than over the boat, and the steamer flow has almost no an effect on the film uniformity.




Line 77: Line 77:


'''
'''
The figure 3 shows that the percent different of silicon dioxide thickness deceases when the process temperature and time increase, which means that the steamer flow rate has less effect on the thicker silicon dioxide film.
The figure 3 shows that the percent different of silicon dioxide thickness deceases when the process temperature and growth time increase, which means that the steamer flow rate has less effect on the thicker silicon dioxide film.


'''
'''

Revision as of 13:58, 1 October 2014

THIS PAGE IS UNDER CONSTRUCTION

Feedback to this page: click here


The wet oxidation by Anneal Oxide Furnace(C1) can be used for growing silicon dioxide by using steamer (RASIRC Steam Generator ), which gives a very good film uniformity. The advantage of this furnace is the brand new wafers no need RCA clean before.


Calculation for wet oxidation

The following links give an approximate oxide time/thickness based on prediction equations from the following experiments:

Calculation for wet oxidation

Test of the wet oxidation by steamer

Purpose

To study the effect of the process temperature, growth time and steamer flow rate on the silicon dioxide thickness and the percent of film non-uniformity. To form the prediction equations, which be able to calculate the growth time from the expected oxide thickness, or calculate the oxide thickness from the growth time.

Experimental setup (1) Effect screening

The boat was fully filled with dummy wafers, and there are three tested wafers per run. The three tested wafers were placed at slot number 6, 15 and 24. The average silicon dioxide thickness and the percent of film non-uniformity over the boat were calculated form those three test wafers. The average silicon dioxide thickness and the percent of film non-uniformity over the wafer was calculated from the wafer slot no.15, which was placed in the middle of the boat. Silicon dioxide thickness was measured 5 points over the wafer by Filmtek.

Pressure: Atmosphere

Temperature: 1000, 1050, 1100 C

Time: 15, 180, 360, 720 minutes

Steamer Flow Rate: 10, 17.5, 25 L/min

Anneal: Same as process temperature for 20 minutes with N2: 6 SLM

Test Wafers: N-Type <100> No RCA Clean

Results (1)

The figure 1 shows that the silicon dioxide thickness over the boat is affected the most by growth time, temperature and steamer flow rate respectively. When the growth time, temperature and steamer flow rate increase, the silicon dioxide thickness also increases. Since the steamer flow has the least an effect to the silicon dioxide thickness, so the flow rate has been fixed at 10 liters per minutes in the furnace recipe.


The average silicon dioxide thickness and the percent of film non-uniformity over the boat variation with process time, steamer flow rate and temperature.

Figure 1. The average silicon dioxide thickness and the percent of film non-uniformity over the boat variation with process time, steamer flow rate and temperature.


The percent of film non-uniformity over the boat most likely depends on the silicon dioxide thickness. The thicker silicon dioxide gives better film uniformity. The figure 1 shows that the percent of film non-uniformity over the boat decreases, when the growth time, steamer flow rate and the temperature increase.


The average silicon dioxide thickness and the percent of film non-uniformity over the wafer variation with growth time, steamer flow rate and temperature.

Figure 2. The average silicon dioxide thickness and the percent of film non-uniformity over the wafer variation with growth time, steamer flow rate and temperature.


The effect of the steamer flow rate, growth time and temperature to the silicon dioxide thickness and to the percent of film non-uniformity over the wafer is quite similar with over the boat. But the percent of film non-uniformity over the boat is lower than over the boat, and the steamer flow has almost no an effect on the film uniformity.


The percent different of the silicon dioxide thickness at the steamer flow rate at 10 and 25 l/min variation with temperature.

Figure 3. The percent different of the silicon dioxide thickness at the steamer flow rate at 10 and 25 l/min variation with temperature.


The figure 3 shows that the percent different of silicon dioxide thickness deceases when the process temperature and growth time increase, which means that the steamer flow rate has less effect on the thicker silicon dioxide film.

Experimental setup (2) Steamer flow rate has been fixed at 10 liter/minutes

The steamer flow rate has been fixed at 10 liter per minutes. The test was done in difference growth time and temperatures.

Pressure: Atmosphere

Temperature: 1000, 1050, 1100 C

Time: 0, 5, 15, 100, 180, 250, 360, 720 minutes

Steamer Flow Rate: 10 L/min

Anneal: Same as process temperature for 20 minutes with N2: 6 SLM

Test Wafers: N-Type <100> No RCA Clean

Results (2)

Figure 4 shows the oxide thickness as a function of oxidation time in three process temperatures. The oxide grows faster at the higher temperature. The prediction equations of each process temperature can be form by this plots, which are based on this experiment in our specific furnaces and give more accurate results. Calculation for wet oxidation


Silicon dioxide thickness variation with growth time (from 0 to 720 minutes) in different temperature.

Figure 4. Silicon dioxide thickness variation with growth time (from 0 to 720 minutes) in different temperature.


The percent of film non-uniformity variation with growth time in different temperature. (left) Over the boat and (right) over the wafer.

Figure 5. The percent of film non-uniformity variation with growth time in different temperature. (left) Over the boat and (right) over the wafer


From figure 5 shows that the percent of film non-uniformity deceases when the process time and process temperature increase. From this experiment, show that the silicon dioxide has a very good uniformity. The percent of film non-uniformity is lower than 1.5 over the boat, and lower than 1.2 over the wafer.