Jump to content

Specific Process Knowledge/Lithography/CSAR: Difference between revisions

From LabAdviser
Tigre (talk | contribs)
Tigre (talk | contribs)
Line 277: Line 277:


== SEM pictures ==
== SEM pictures ==
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 60%;"
|-
|-
|-style="background:Black; color:White"
!Equipment
!Process Parameters
!Comments
|-
|-
|-style="background:LightGrey; color:black"
|4" Si wafers
|No Pretreatment
|
|-
|-
|-style="background:LightGrey; color:black"
|Spin Coater Manual, LabSpin, A-5
|AR-P 6200/2 AllResist E-beam resist
60 sec at various spin speed.
Acceleration 4000 s-2,
softbake 1 - 5 min at 150 deg Celcius
|Disposal pipette used; clean by N2-gun before use. Use approximately 1.5 ml per 4" wafer, never use a pipette twice. Softbake is not a crucial step, see e-mail correspondence with AllResist [[media:Softbake CSAR.pdf|here]].
|-
|-
|-style="background:LightGrey; color:black"
|Ellipsometer VASE B-1
|9 points measured on 100 mm wafer
|ZEP program used; measured at 70 deg only
|-
|-
|-style="background:LightGrey; color:black"
|JEOL 9500 E-beam writer, E-1
|Dosepattern 15nm - 100nm,
dose 120-280 muC/cm2
|Virtual chip mark height detection (CHIPAL V1) used in corner of every dose array
|-
|-
|-style="background:LightGrey; color:black"
|Fumehood, D-3
|60 sec in X AR 600-54/6,
60 sec rinse in IPA,
N2 Blow dry
|Gentle agitation while developing. After developing, wafer is immersed in beaker with IPA, subsequently blow dried with N2 gun.
|-
|-
|-style="background:LightGrey; color:black"
|Zeiss SEM Supra 60VP, D-3
|2 kV, shortest working distance possible, chip mounted with Al tape
|Before characterization, wafers were sputter coated with 2-3 nm Pt at DTU CEN.
|-
|}


The wafers are diced into smaller pieces and sputter coated with Pt at DTU CEN before SEM inspection; please contact [mailto:ramona.mateiu@cen.dtu.dk|Ramona Valentina Mateiu] for further information.
The wafers are diced into smaller pieces and sputter coated with Pt at DTU CEN before SEM inspection; please contact [mailto:ramona.mateiu@cen.dtu.dk|Ramona Valentina Mateiu] for further information.

Revision as of 12:08, 7 July 2014

These tests are currently in progress and this page thus under construction. If you have questions to the process or wish to use this e-beam resist, please contact Tine Greibe at tigre@danchip.dtu.dk.


Process Flow

Test of Chemically Semi-Amplified Resist (CSAR); a positive e-beam resist from AllResist (AR-P 6200-2).

Equipment Process Parameters Comments
Pretreatment
4" Si wafers No Pretreatment
Spin Coat
Spin Coater Manual, LabSpin, A-5 AR-P 6200/2 AllResist E-beam resist

60 sec at various spin speed. Acceleration 4000 s-2, softbake 1 - 5 min at 150 deg Celcius

Disposal pipette used; clean by N2-gun before use. Use approximately 1.5 ml per 4" wafer, never use a pipette twice. Softbake is not a crucial step, see e-mail correspondence with AllResist here.
Characterization
Ellipsometer VASE B-1 9 points measured on 100 mm wafer ZEP program used; measured at 70 deg only
E-beam Exposure
JEOL 9500 E-beam writer, E-1 Dosepattern 15nm - 100nm,

dose 120-280 muC/cm2

Virtual chip mark height detection (CHIPAL V1) used in corner of every dose array
Development
Fumehood, D-3 60 sec in X AR 600-54/6,

60 sec rinse in IPA, N2 Blow dry

Gentle agitation while developing. After developing, wafer is immersed in beaker with IPA, subsequently blow dried with N2 gun.
Characterization
Zeiss SEM Supra 60VP, D-3 2 kV, shortest working distance possible, chip mounted with Al tape Before characterization, wafers were sputter coated with 2-3 nm Pt at DTU CEN.

Spin Curves

The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.

AllResist AR-P 6200/2 spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 09-04-2014. Softbake 5 min @ 150 degC.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
2000 4000 225.98 0.97
3000 4000 194.00 0.6
4000 4000 169.57 0.32
5000 4000 151.47 0.26
6000 4000 142.38 0.41
7000 4000 126.59 0.36


AllResist CSAR on Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
3000 4000 201.61 1.20
4000 4000 173.89 0.64
5000 4000 155.91 0.65


AllResist CSAR 1:1 in anisole, Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
2000 4000 83.48 0.49
3000 4000 67.12 0.41
4000 4000 58.64 0.44
5000 4000 53.13 0.39
6000 4000 48.76 0.38


SEM pictures

Equipment Process Parameters Comments
4" Si wafers No Pretreatment
Spin Coater Manual, LabSpin, A-5 AR-P 6200/2 AllResist E-beam resist

60 sec at various spin speed. Acceleration 4000 s-2, softbake 1 - 5 min at 150 deg Celcius

Disposal pipette used; clean by N2-gun before use. Use approximately 1.5 ml per 4" wafer, never use a pipette twice. Softbake is not a crucial step, see e-mail correspondence with AllResist here.
Ellipsometer VASE B-1 9 points measured on 100 mm wafer ZEP program used; measured at 70 deg only
JEOL 9500 E-beam writer, E-1 Dosepattern 15nm - 100nm,

dose 120-280 muC/cm2

Virtual chip mark height detection (CHIPAL V1) used in corner of every dose array
Fumehood, D-3 60 sec in X AR 600-54/6,

60 sec rinse in IPA, N2 Blow dry

Gentle agitation while developing. After developing, wafer is immersed in beaker with IPA, subsequently blow dried with N2 gun.
Zeiss SEM Supra 60VP, D-3 2 kV, shortest working distance possible, chip mounted with Al tape Before characterization, wafers were sputter coated with 2-3 nm Pt at DTU CEN.

The wafers are diced into smaller pieces and sputter coated with Pt at DTU CEN before SEM inspection; please contact Valentina Mateiu for further information.

50nm

dose [muC/cm2] 207 219 230 242


30nm

dose [muC/cm2] 207 219 230 242