Jump to content

Specific Process Knowledge/Etch/KOH Etch: Difference between revisions

From LabAdviser
Fj (talk | contribs)
Fj (talk | contribs)
Line 3: Line 3:
KOH belongs to the family of anisotropic Si-etchants based on aqueous alkaline solutions. The anisotropy stems from the different etch rates in different crystal directions. The {111}-planes are almost inert whereas the etch rates of e.g. {100}- and {110}-planes are several orders of magnitude faster.
KOH belongs to the family of anisotropic Si-etchants based on aqueous alkaline solutions. The anisotropy stems from the different etch rates in different crystal directions. The {111}-planes are almost inert whereas the etch rates of e.g. {100}- and {110}-planes are several orders of magnitude faster.


At Danchip we use as a standard a 28 wt% KOH. The etch rate - and the selectivity towards a SiO2-mask - is depending on the temperature. We normally use T=80 <sup>o</sup>C but may choose to reduce this to e.g. 60 <sup>o</sup>C or 70 <sup>o</sup>C in case of a high-precission timed etch (e.g. defining a thin membrane). In some cases we recommend to saturate the standard 28 wt%KOH with IPA with T=70 <sup>o</sup>C (reduce evaporation of IPA). One example is for boron etch-stop, where the selectivity towards the boron-doped silicon is improved.  
At Danchip we use as a standard a 28 wt% KOH. The etch rate - and the selectivity towards a SiO<math>_2</math>-mask - is depending on the temperature. We normally use T=80 <sup>o</sup>C but may choose to reduce this to e.g. 60 <sup>o</sup>C or 70 <sup>o</sup>C in case of a high-precission timed etch (e.g. defining a thin membrane). In some cases we recommend to saturate the standard 28 wt%KOH with IPA with T=70 <sup>o</sup>C (reduce evaporation of IPA). One example is for boron etch-stop, where the selectivity towards the boron-doped silicon is improved.  


<br clear="all" />
<br clear="all" />

Revision as of 12:21, 28 January 2008

KOH etch - Anisotropic silicon etch

KOH etch for 4" wafers: positioned in cleanroom 3

KOH belongs to the family of anisotropic Si-etchants based on aqueous alkaline solutions. The anisotropy stems from the different etch rates in different crystal directions. The {111}-planes are almost inert whereas the etch rates of e.g. {100}- and {110}-planes are several orders of magnitude faster.

At Danchip we use as a standard a 28 wt% KOH. The etch rate - and the selectivity towards a SiO2-mask - is depending on the temperature. We normally use T=80 oC but may choose to reduce this to e.g. 60 oC or 70 oC in case of a high-precission timed etch (e.g. defining a thin membrane). In some cases we recommend to saturate the standard 28 wt%KOH with IPA with T=70 oC (reduce evaporation of IPA). One example is for boron etch-stop, where the selectivity towards the boron-doped silicon is improved.


Comparing the two solutions

Aluminium Etch 1 Aluminium Etch 2
General description

Etch of pure aluminium

Etch of aluminium + 1.5% Si

Chemical solution H2O:H3PO4 1:2 PES 77-19-04
Process temperature 50 oC 20 oC
Possible masking materials:

Photoresist (1.5 µm AZ5214E)

Photoresist (1.5 µm AZ5214E)

Etch rate

~100 nm/min (Pure Al)

~60(??) nm/min

Batch size

1-25 wafers at a time

1-25 wafer at a time

Size of substrate

4" wafers

4" wafers

Allowed materials
  • Aluminium
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resist
  • Aluminium
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resist