Specific Process Knowledge/Etch/Wet Gold Etch: Difference between revisions
| Line 11: | Line 11: | ||
# Iodine etch: KI:I<sub>2</sub>:H<sub>2</sub>O - 100g:25g:500ml - standard at Danchip. Can be used with AZ resist as mask. | # Iodine etch: KI:I<sub>2</sub>:H<sub>2</sub>O - 100g:25g:500ml - standard at Danchip. Can be used with AZ resist as mask. | ||
# Aqua Regia (Kongevand): HNO<sub>3</sub>:HCl - 1:3 - A very strong acid | # Aqua Regia (Kongevand): HNO<sub>3</sub>:HCl - 1:3 - A very strong acid which will etch most metals and are therefore used when you wish to remove all the gold from your wafer. '''you have to be very carefull when you work with Aqua Regia (Kongevand) It can generate nitrous gases witch are very toxic!!''' | ||
Revision as of 14:39, 7 May 2014
Feedback to this page: click here
Ething of Gold can be done either wet or dry. For wet etching please see below on this page. Dry etching can be done with IBE by sputtering with Ar ions.
Etching of Gold

Etching of Gold is done wet at Danchip making your own set up in a beaker in the fumehood. You can see the APV here.
We have two different solutions:
- Iodine etch: KI:I2:H2O - 100g:25g:500ml - standard at Danchip. Can be used with AZ resist as mask.
- Aqua Regia (Kongevand): HNO3:HCl - 1:3 - A very strong acid which will etch most metals and are therefore used when you wish to remove all the gold from your wafer. you have to be very carefull when you work with Aqua Regia (Kongevand) It can generate nitrous gases witch are very toxic!!
Comparing the two solutions
| Iodine based gold etch | Aqua Regia (Kongevand) | |
|---|---|---|
| General description |
Etch of pure Gold with or without photoresist mask. |
Etch of pure Gold (as stripper). |
| Link to safety APV | see APV here. | see APV here |
| Chemical solution | KI:I2:H2O (100g:25g:500ml) | HCl:HNO3 (3:1) |
| Process temperature | 20 oC | 20 oC |
| Possible masking materials |
Photoresist (1.5 µm AZ5214E) |
Unmasked - used as a stripper |
| Etch rate |
~100 nm/min |
~(??) nm/min - fast etch |
| Batch size |
1-5 4" wafers at a time |
1-5 4" wafer at a time |
| Size of substrate | Any size and number that can go inside the beaker in use | Any size and number that can go inside the beaker in use |
| Allowed materials |
No restrictions when used in beaker. Make a note on the beaker of which materials have been processed. |
No restrictions when used in beaker. Make a note on the beaker of which materials have been processed. |