| ==Comparison of the methods for deposition of Silicon Oxide== | | ==Comparison of the methods for deposition of Silicon Oxide== |
| {| border="1" cellspacing="0" cellpadding="4" align="center"
| |
| !
| |
| ! LPCVD (TEOS)
| |
| ! PECVD
| |
| ! Sputter technique [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon oxide in PVD co-sputter/evaporation|(PVD co-sputter/evaporation tool)]]
| |
| !Sputter technique using [[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE/IBSD Ionfab300]]
| |
| |- valign="top" align="left"
| |
| | Stochiometry
| |
| |
| |
| *SiO<sub>2</sub>
| |
| Can be doped with boron
| |
| |
| |
| *Si<sub>x</sub>O<sub>y</sub>H<sub>z</sub>
| |
| Can be doped with boron, phosphorus or germanium
| |
| |
| |
| *Not measured (a sputter target with stoichiometry SiO<sub>2</sub> is used)
| |
| |
| |
| *Not measured (a sputter target with stoichiometry SiO<sub>2</sub> is used
| |
| |-valign="top" align="left"
| |
| |Film thickness
| |
| |
| |
| *~300nm - 4µm
| |
| |
| |
| *~40nm - 30µm
| |
| |
| |
| *Thin layers (up to 300-400 nm)
| |
| |
| |
| *~10nm - ~1µm(>2h)
| |
| |- valign="top" align="left"
| |
| |Process Temperature
| |
| |
| |
| *725 <sup>o</sup>C
| |
| |
| |
| *300 <sup>o</sup>C
| |
| |
| |
| *Can be between room temp. and 400 <sup>o</sup>C
| |
| |
| |
| *Expected to be below 100<sup>o</sup>C
| |
| |- valign="top" align="left"
| |
| |Step coverage
| |
| |
| |
| *Excelent. Very high surface mobility.
| |
| |
| |
| *Less good
| |
| *When doped with phosphorus and/or Boron the oxide can float at about 1000 <sup>o</sup>C in a wet oxidation.
| |
| |
| |
| *
| |
| |Not Known
| |
| |- valign="top" align="left"
| |
| |Film quality
| |
| |
| |
| *Less than thermal oxide. Annealing makes it more dense.
| |
| *Few defects
| |
| |
| |
| *Less dense film
| |
| *Incorporation of hydrogen in the film
| |
| |
| |
| *
| |
| |
| |
| *
| |
| |- valign="top" align="left"
| |
| |Batch size
| |
| |
| |
| *1-13 4" wafer per run
| |
| *deposition on both sides of the substrate
| |
| |
| |
| *1-3 4" wafers or 1 6" wafer or many smaller chips per run
| |
| *deposition on one side of the substrate
| |
| |
| |
| *1-12 4" wafers or 1-4 6" wafer or many smaller chips per run
| |
| *Deposition time for 1 and 3 wafers is the same
| |
| |
| |
| *1 50mm wafer
| |
| *1 100mm wafer
| |
| *1 150mm wafer
| |
| *1 200mm wafer
| |
| *Smaller pieces can be mounted with capton tape
| |
| |- valign="top" align="left"
| |
| | Substrate material allowed
| |
| |
| |
| *Silicon wafers
| |
| **with layers of silicon oxide or silicon (oxy)nitride
| |
| *Quartz wafers
| |
| |
| |
| *Silicon
| |
| **with layers of silicon oxide or silicon (oxy)nitride
| |
| *Quartz
| |
| *Small amount of metal (in PECVD3)
| |
| |
| |
| *Silicon
| |
| **with layers of silicon oxide or silicon (oxy)nitride
| |
| *Quartz
| |
| *Metals
| |
| |
| |
| *Almost any materials
| |
| *not Pb and very poisonous materials
| |
| |-
| |
| |}
| |
|
| |
| {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" |
| |- | | |- |
Feedback to this page: click here
Deposition of Silicon Oxide can be done with either LPCVD, PECVD or by sputter technique. You can also make a silicon oxide layer by growing a thermal oxide in a hot furnace but that requires a silicon surface as a starting point.
Deposition of Silicon Oxide using LPCVD
The LPCVD oxide you can deposit at DANCHIP is called TEOS oxide. It can be made in the LPCVD TEOS furnace. It is a batch process meaning you can run a batch of 13 wafers at a time. The deposition takes place at temperatures of 725 degrees Celsius. The TEOS oxide has good step coverage and hole filing/covering properties and the film thickness is very uniform over the wafer. We have two standard TEOS processes: One for depositing standard layers ~(0-1.5 µm) and one for deposition thick layers ~(1.5µm-4µm). The TEOS oxide has a dielectric constant very close to the one for thermal oxide (3.65 for TEOS).
Deposition of Silicon Oxide using PECVD
PECVD oxide can be deposited in one of the PECVD systems. You can run 1-3 wafers at a time depending on which one of the PECVD's you use. The deposition takes place at 300 degrees Celcius. This can be of importance for some applications but it gives a less dense film and the oxide is expected to have some hydrogen incorporated. The step coverage and thickness uniformity of the film is not as good as for the LPCVD TEOS oxide. PECVD oxide has excellent floating properties when doped with boron and/or phosphorus. Then it can be used ex. as top cladding for waveguides or encapsulation of various structures/components. In one of our PECVD systems (PECVD3) we allow small amounts of metal on the wafers entering the system, this is not allowed in the LPCVD and in the other PECVD (PECVD1). It is also a possibility to dope the silicon oxide with Germanium for altering the refractive index of the oxide.
Deposition of Silicon Oxide using sputter deposition technique
At DANCHIP you can also deposit silicon oxide using Lesker, PVD co-sputter/evaporation or IBE Ionfab300
sputter systems. One of the advantages here is that you can deposit on any material you like.
Comparison of the methods for deposition of Silicon Oxide
|
|
LPCVD(TEOS)
|
PECVD
|
PVD co-sputter/evaporation tool
|
IBE/IBSD Ionfab300
|
| Generel description
|
Generel description - method 1
|
Generel description - method 2
|
.
|
.
|
| Stochiometry
|
Can be doped with boron
|
Can be doped with boron, phosphorus or germanium
|
- Not measured (a sputter target with stoichiometry SiO2 is used)
|
- Not measured (a sputter target with stoichiometry SiO2 is used
|
| Film thickness
|
|
|
- Thin layers (up to 300-400 nm)
|
|
| Process Temperature
|
|
|
- Can be between room temp. and 400 oC
|
- Expected to be below 100oC
|
| Step Coverage
|
- Excelent. Very high surface mobility.
- Deposition on both sides of the substrate.
|
- Less good
- When doped with phosphorus and/or Boron the oxide can float at about 1000 oC in a wet oxidation.
- Deposition on one side of the substrate
|
- Not known
- Deposition on one side of the substrate
|
- Not Known
- Deposition on one side of the substrate
|
| Film Quality
|
- Less than thermal oxide. Annealing makes it more dense.
- Few defects
|
- Less dense film
- Incorporation of hydrogen in the film
|
|
|
| Substrate size / Batch size
|
|
- Several small samples
- 1-7 50 mm wafers
- 1-3 100 mm wafers
- 1 150 mm wafer
|
- Several small samples
- 1-12 100 mm wafers
- 1-4 150 mm wafers
- Process time for 3 wafers is the same as for 1 wafer
|
- Several small samples mounted with capton tape
- 1 50 mm wafer
- 1 100 mm wafer
- 1 150 mm wafer
- 1 200 mm wafer
|
| Allowed materials
|
- Silicon wafers
- with layers of silicon oxide or silicon (oxy)nitride
- Quartz wafers
|
- Silicon
- with layers of silicon oxide or silicon (oxy)nitride
- Quartz
- IIIV materials (in PECVD2)
- Small amount of metal (in PECVD3)
|
- Silicon
- with layers of silicon oxide or silicon (oxy)nitride
- Quartz
- Metals
|
- Almost any material
- not Pb and very poisonous materials
|