Jump to content

Specific Process Knowledge/Etch/Wet Polysilicon Etch: Difference between revisions

From LabAdviser
Kabi (talk | contribs)
No edit summary
Kabi (talk | contribs)
Line 15: Line 15:
'''NB: The life time of the solution is only a few days.'''
'''NB: The life time of the solution is only a few days.'''


'''The user manual and contact information can be found in LabManager:'''
<!-- remember to remove the type of documents that are not present -->
[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=129 Isotropic Etch/Poly Etch info page in LabManager]


===PolySi Etch data===
===PolySi Etch data===

Revision as of 12:46, 21 February 2014

Feedback to this page: click here

Wet PolySi Etch

Wet PolySilicon Etch (in the middle): positioned in cleanroom 4

The wet PolySi Etch is an isotropic silicon etch. This holds for both a poly-silicon thin-film as well as single-crystalline material such as a Si(100) surface. The PolySi Etch process is placed in a dedicated PP-tank in a laminar-flow bench in cleanroom 4.

The PolySi Etch is typically used for opening holes in poly-silicon thin-films, using photoresist as an etch mask. Due to its isotropic nature the under-etching (etch-bias) at least amounts to the thickness of the poly-silicon layer. Another example of usage is etching of "circular-shaped" holes in silicon substrates.

The PolySi Etch is based on the combined oxidation of silicon followed by dissolution of the silicon oxide. The etch solution consists of:

HNO3 : BHF : H2O - (20 : 1 : 20)

NB: The life time of the solution is only a few days.

The user manual and contact information can be found in LabManager:

Isotropic Etch/Poly Etch info page in LabManager

PolySi Etch data

PolySi Etch @ room temperature
General description

Etch of poly-si/Si(100)

Chemical solution HNO3 : BHF : H2O (20 : 1 : 20)
Process temperature Room temperature
Possible masking materials
  • Photoresist(min. 2.2 µm is recommended)
  • LPCVD-oxide (TEOS)
Etch rate
  • RSi ~1000-2000 Å/min (depending on doping level)
  • RSiO2 ~60 Å/min
  • Photoresist (2.2 µm) withstand ~20-30 min
Batch size

1-25 wafers at a time

Size of substrate

2-4" wafers