Specific Process Knowledge/Etch/ICP Metal Etcher/silicon oxide: Difference between revisions
Appearance
| Line 47: | Line 47: | ||
|[[image:ICP_metal_slow_wafer_uniformity_s4075.jpg|275x275px|right|thumb|Contour plot of the etch rate over the wafer, 9 points measured]] | |[[image:ICP_metal_slow_wafer_uniformity_s4075.jpg|275x275px|right|thumb|Contour plot of the etch rate over the wafer, 9 points measured]] | ||
|- | |- | ||
| | |SEM profile images | ||
| | | | ||
<gallery caption="Some chemicals of the MVD and the surface reaction" widths="200px" heights="150px" perrow="3"> | |||
image:ICP_metal_resist_no_etch_s4075_2.jpg|Resist profile before etch | |||
image:ICP_metal_slow_s4075_sio2_4.jpg|Resist profiler after etch 01-02-2014. | |||
image:ICP_metal_slow_s4075_sio2_6.jpg|Resist profiler after etch 01-02-2014. No line width reduction observed. | |||
</gallery> | |||
|- | |- | ||
|} | |} | ||
<br/> | <br/> | ||
Revision as of 11:18, 17 February 2014
Slow etch of SiO2 with resist as masking material - with direct clamping 
This recipe can be used for slow etching of SiO2 with resist as masking material when normal clamping is possible. Normal clamping is prefered because it give the best and most repeatable cooling of the wafer. Here are some test results presented.
| Parameter | Resist mask |
|---|---|
| Coil Power [W] | 200 |
| Platen Power [W] | 25 |
| Platen temperature [oC] | 0 |
| CF4 flow [sccm] | 20 |
| H2 flow [sccm] | 10 |
| Pressure [mTorr] | 3 |