Specific Process Knowledge/Etch/Wet Aluminium Etch: Difference between revisions
Line 7: | Line 7: | ||
# Pre-mixed etch solution: PES 77-19-04 at 20 <sup>o</sup>C | # Pre-mixed etch solution: PES 77-19-04 at 20 <sup>o</sup>C | ||
<br clear="all" /> | |||
===Comparing the two solutions=== | ===Comparing the two solutions=== | ||
Revision as of 10:56, 15 January 2008
Wet Aluminium Etch

Wet etching of aluminium is done with two different solutions:
- HO:HPO 1:2 at 50 oC
- Pre-mixed etch solution: PES 77-19-04 at 20 oC
Comparing the two solutions
Aluminium Etch 1 | Aluminium Etch 2 | |
---|---|---|
General description |
Etch of pure aluminium |
Etch of aluminium + 1.5% Si |
Chemical solution | HO:HPO 1:2 | PES 77-19-04 |
Process temperature | 50 oC | 20 oC |
Possible masking materials: |
Photoresist (1.5 µm AZ5214E) |
Photoresist (1.5 µm AZ5214E) |
Etch rate |
~100 nm/min (Pure Al) |
~60(??) nm/min |
Batch size |
1-25 wafers at a time |
1-25 wafer at a time |
Size of substrate |
4" wafers |
4" wafers |
Allowed materials |
|
|