The measured standard is 0.1 mm. The measured result have to be within +- 0.005 mm. The QC is preformed ones a year.
The measured standard thickness is 0.1 mm. The measured result have to be within +- 0.005 mm. The QC is preformed ones a year.
|}
|}



Revision as of 12:06, 13 January 2014

THIS PAGE IS UNDER CONSTRUCTION

Feedback to this page: click here

Thickness measurer

File:??.jpg
Thickness meassurer. Positioned in cleanroom 4

The purpose is to measure the thickness of wafers, depths of larger grooves or height of larger mesas.

Doing a KOH etch can it be helpful to insure no over etching by making a thickness measurement doing the etch.

The user manual, technical information and contact information can be found in LabManager:

Thickness measurer

Process knowledge

Quality Control - Recipe Parameters and Limits

Quality Control (QC) for the Thickness measurer

The measured standard thickness is 0.1 mm. The measured result have to be within +- 0.005 mm. The QC is preformed ones a year.

Equipment performance and process related parameters

Purpose

Measurer the thinkness of silicon wafer

??

Performance

??

??

Process parameter range

Process Temperature

  • 800-1150 oC
Process pressure
  • 1 atm
Gasses on the system
Substrates Batch size
  • 1-30 100 mm wafers (or 50 mm wafers) per run
Substrate materials allowed
  • Silicon wafers (RCA cleaned) without metal bulk contamination