Specific Process Knowledge/Etch/Etching of SU-8: Difference between revisions

From LabAdviser
Khara (talk | contribs)
No edit summary
Khara (talk | contribs)
No edit summary
Line 4: Line 4:
* High anisotropic etch: etch rate ~400nm/min, anisotropy ~0.8
* High anisotropic etch: etch rate ~400nm/min, anisotropy ~0.8
* Low anisotropic etch: etch rate ~180nm/min, anisotropy ~0.3
* Low anisotropic etch: etch rate ~180nm/min, anisotropy ~0.3
==Recipes in ASE==
===SU8aniso===
The anisotropic SU8aniso etch was design to etch structures in SU-8 with a low roughness of the etched surface, however it has not been tested with any mask material. For a polymeric mask a low selectivity is expected. The etch rate was measured to around 400 nm/min, but will depend on wafer coverage. The surface layer concentration of antimony (Sb) after etch is expected to be below 2%.
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
|+ '''SU8aniso etch''' by khara@danchip
|-
! Parameter
|'''SU8aniso etch'''
|-
! O<sub>2</sub> (sccm)
| 99
|-
! SF<sub>6</sub> (sccm)
| 17
|-
! Pressure (mTorr)
| 40
|-
! Coil power (W)
| 800
|-
! Platen power (W)
| 30
|-
! Temperature (<sup>o</sup>C)
| 30
|-
! Etch rate (nm/min)
| ~400
|-
!anisotropy
|~0.8
|}
===SU8iso

Revision as of 09:26, 4 November 2013

Etching of SU-8

SU-8 can be etched by a oxygen plasma with a small amount of SF6 to remove the antimony present from the photo initiator. Etching of SU-8 has been developed on the ASE and was tested as a mask less reduction of pattern defined by photo lithography. Two processes are available, a high and a low anisotropic etch for use as etching or thinning of structures.

  • High anisotropic etch: etch rate ~400nm/min, anisotropy ~0.8
  • Low anisotropic etch: etch rate ~180nm/min, anisotropy ~0.3

Recipes in ASE

SU8aniso

The anisotropic SU8aniso etch was design to etch structures in SU-8 with a low roughness of the etched surface, however it has not been tested with any mask material. For a polymeric mask a low selectivity is expected. The etch rate was measured to around 400 nm/min, but will depend on wafer coverage. The surface layer concentration of antimony (Sb) after etch is expected to be below 2%.

SU8aniso etch by khara@danchip
Parameter SU8aniso etch
O2 (sccm) 99
SF6 (sccm) 17
Pressure (mTorr) 40
Coil power (W) 800
Platen power (W) 30
Temperature (oC) 30
Etch rate (nm/min) ~400
anisotropy ~0.8