! E-beam evaporation (Leybold)
! E-beam evaporation (Leybold)
! E-beam evaporation (Wordentec)
! E-beam evaporation (Wordentec)
! Sputter deposition (Wordentec)
|-  
|-  
| Batch size
| Batch size
Line 15: Line 16:
*8x4" wafers or
*8x4" wafers or
*5x6" wafers
*5x6" wafers
|
*24x2" wafers or
*6x4" wafers or
*6x6" wafers
|
|
*24x2" wafers or  
*24x2" wafers or  
Line 23: Line 28:
|RF Ar clean
|RF Ar clean
|Ar ion bombartment
|Ar ion bombartment
|RF Ar clean
|RF Ar clean
|RF Ar clean
|-
|-
Line 29: Line 35:
|10Å to 0.5µm
|10Å to 0.5µm
|10Å to 1 µm
|10Å to 1 µm
|.
|-
|-
| Deposition rate
| Deposition rate
Line 34: Line 41:
|1Å/s to 5Å/s
|1Å/s to 5Å/s
|10Å/s to 15Å/s
|10Å/s to 15Å/s
|.
|-
|-
|}
|}

Revision as of 12:37, 19 December 2007

Titanium can be deposited by e-beam evaporation. In the chart below you can compare the different deposition equipment.


E-beam evaporation (Alcatel) E-beam evaporation (Leybold) E-beam evaporation (Wordentec) Sputter deposition (Wordentec)
Batch size
  • Up to 1x4" wafers
  • smaller pieces
  • 8x4" wafers or
  • 5x6" wafers
  • 24x2" wafers or
  • 6x4" wafers or
  • 6x6" wafers
  • 24x2" wafers or
  • 6x4" wafers or
  • 6x6" wafers
Pre-clean RF Ar clean Ar ion bombartment RF Ar clean RF Ar clean
Layer thickness 10Å to 1µm 10Å to 0.5µm 10Å to 1 µm .
Deposition rate 2Å/s to 15Å/s 1Å/s to 5Å/s 10Å/s to 15Å/s .