!Etch rate range | !Etch rate range | ||
| | | | ||
* | *~75 nm/min (Thermal oxide) in BHF | ||
| | *~90 nm/min (Thermal oxide) in SIO Etch | ||
*~25 nm/min (Thermal oxide) in 5%HF | |||
*~3-4µm/min in 40%HF| | |||
*Typically 40-50 nm/min can be increased or decreased by using other recipe parameters. | *Typically 40-50 nm/min can be increased or decreased by using other recipe parameters. | ||
| | | | ||
Revision as of 16:53, 11 April 2013
Silicon oxide can be etched using either wet chemistry or dry etch equipment. Wet chemistry is mainly used to remove all the oxide on the surface (backside and front side) of a wafer or for isotrotropic etching. Dry etching etches anisotropic. It etches one side of the wafer at a time and can be used to etch structures with several masking materials.
Etch of silicon oxide can be done by either wet etch or dry etch. The standard setups for this here at DANCHIP are:
Wet etches:
Dry etches:
Comparison of wet Silicon Oxide etch and dry etches (RIE and AOE) etch for etching of Silicon Oxide
| Wet Silicon Oxide etch (BHF, SIO Etch (wetting agent), 5%HF) | RIE | AOE | |
|---|---|---|---|
| General description |
|
|
|
| Possible masking materials |
|
|
|
| Etch rate |
|
|
|
| Batch size |
|
|
|
| Size of substrate |
|
|
|
| Allowed materials |
|
|
|
This Part is under construction
Feedback to this page: click here
Comparing silicon oxide etch methods at Danchip 
There are a broad varity of silicon oxide etch methods at Danchip. The methodes are compared here to make it easier for you to compare and choose the one that suits your needs.
Compare the methods for Silicon Oxide etching
| Wet Silicon Oxide etch (BHF/HF) | RIE (Reactive Ion Etch) | AOE (Advanced Oxide Etch) | IBE/IBSD Ionfab 300 | |
|---|---|---|---|---|
| Generel description |
|
|
|
|
| Possible masking materials |
|
|
AOE
|
|
| Etch rate range |
|
AOE |
| |
| Substrate size |
|
|
|
|
| Allowed materials |
|
|
|
|