Wet etching of Chromium

Wet Etch of Chromium can take place in a beaker in this fume hood
Wet etching of chromium at Danchip is done making your own set up in a beaker in a fume hood - preferably in cleanroom 2 or 4. We have two solution for this:
- HNO3:H2O:cerisulphate - 90ml:1200ml:15g - standard at Danchip
- Commercial chromium etch
Etch rate are depending on the level of oxidation of the metal.
How to mix the Chromium etch 1:
- Take a beaker and add 15g of cerisulphate.
- Add a little water while stirring - make sure all lumps are gone.
- Add water until 600 ml - keep stirring (use magnetic stirring)
- Add 90 ml HNO3
- When the cerisulphate is completely dissolved (clear liquid) you can add the other 600 ml of wafer.
Overview of the data for the chromium etches
| Chromium etch 1 | Chromium etch 2 | |
|---|---|---|
| General description |
Etch of chromium |
Etch of chromium |
| Link to APV/KBA | ||
| Chemical solution | HNO3:H2O:cerisulphate - 90ml:1200ml:15g | . |
| Process temperature | Room temperature | . |
| Possible masking materials |
Photoresist (1.5 µm AZ5214E) |
. |
| Etch rate |
~40-100 nm/min |
. |
| Batch size |
1-25 wafers at a time |
. |
| Size of substrate |
4" wafers |
. |
| Allowed materials |
No restrictions. Make a note on the bottle of which materials have been processed. |
. |