Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF): Difference between revisions
| Line 10: | Line 10: | ||
===Silicon oxide etch data=== | ===Silicon oxide etch data=== | ||
{| border="2" cellspacing="0" cellpadding="4" align="left" width=" | {| border="2" cellspacing="0" cellpadding="4" align="left" width="900" | ||
! | ! | ||
! BHF | ! BHF | ||
! 5% HF | ! 5% HF | ||
! 40 % HF | |||
! SIO | ! SIO | ||
|- | |- | ||
| Line 21: | Line 22: | ||
| | | | ||
Mainly for removing native oxide | Mainly for removing native oxide | ||
| | |||
Mainly for etching deep into borofloat or quartz wafers | |||
| | | | ||
Etching of silicon oxide - especially for etching small holes | Etching of silicon oxide - especially for etching small holes | ||
| Line 27: | Line 30: | ||
|BHF | |BHF | ||
|5% HF | |5% HF | ||
|40% HF | |||
|BHF with wetting agent | |BHF with wetting agent | ||
|- | |- | ||
|'''Process temperature''' | |'''Process temperature''' | ||
|Room temperature | |||
|Room temperature | |Room temperature | ||
|Room temperature | |Room temperature | ||
| Line 49: | Line 54: | ||
In RCA bench: | In RCA bench: | ||
*No masking material | *No masking material | ||
| | |||
In '''plastic''' beaker with magnetic stirrer in the fume hood in cleanroom 2: | |||
*Photoresist | |||
*Silicon nitride (Only on quartz wafers) | |||
*PolySi(Only on quartz wafers) | |||
*Blue film | |||
*Chromium and gold | |||
| | | | ||
*Photoresist | *Photoresist | ||
| Line 64: | Line 76: | ||
*PECVD1 (standard):~87nm/min | *PECVD1 (standard):~87nm/min | ||
*TEOS:~153nm/min | *TEOS:~153nm/min | ||
| | |||
*Boronfloat and quartz: ~3-4 μm/min | |||
| | | | ||
A little higher etch rates than BHF | A little higher etch rates than BHF | ||
|- | |- | ||
|'''[[#Life_time_of_the_photoresist_and_blue_film_in_BHF|Life time of the photoresist]]''' | |'''[[#Life_time_of_the_photoresist_and_blue_film_in_BHF|Life time of the photoresist]]''' | ||
|~½ hour | |||
|~½ hour | |~½ hour | ||
|~½ hour | |~½ hour | ||
| Line 87: | Line 102: | ||
RCA bench: | RCA bench: | ||
*1-25 wafers of 4" at a time | *1-25 wafers of 4" at a time | ||
| | |||
1-7 wafer of 4" at a time | |||
| | | | ||
1-25 wafer of 4" at a time | 1-25 wafer of 4" at a time | ||
| Line 95: | Line 112: | ||
| | | | ||
2"-6" wafers | 2"-6" wafers | ||
| | |||
4" wafers | |||
| | | | ||
4" wafers | 4" wafers | ||
| Line 112: | Line 131: | ||
In RCA bench: | In RCA bench: | ||
*Only new wafers from the box or during RCA cleaning | *Only new wafers from the box or during RCA cleaning | ||
| | |||
In plastic beaker in the fume hood in cleanroom 2: | |||
*All materials | |||
| | | | ||
*Silicon | *Silicon | ||
Revision as of 17:22, 19 December 2012
Wet Silicon Oxide Etch (BHF and SIO Etch (wetting agent))

Silicon oxide can be etched using HF. At Danchip it is mainly used in a buffered version BHF (premixed). The BHF has a more stable etch rate and is more gentle to photoresist due to an almost pH neutral solution which makes photoresist a good masking material for the oxide etch.
SIO etch (BHF with wetting agent) can also be used for etching silicon oxide. This is mainly for etching small holes. If you have wetting problems in BHF try the SIO etch. It is also a good idea to wet the sample in water for a few minutes before etching.
Wafers with metals or other materials, not allowed in the dedicated oxide etch baths, can be etched in the PP-bath positioned in the fume hood in cleanroom 2 or in a plastic beaker.
Silicon oxide etch data
| BHF | 5% HF | 40 % HF | SIO | |
|---|---|---|---|---|
| General description |
Etching of silicon oxide with a stable etch rate |
Mainly for removing native oxide |
Mainly for etching deep into borofloat or quartz wafers |
Etching of silicon oxide - especially for etching small holes |
| Chemical solution | BHF | 5% HF | 40% HF | BHF with wetting agent |
| Process temperature | Room temperature | Room temperature | Room temperature | Room temperature |
| Possible masking materials |
|
In plastic beaker or PP-bath in the fume hood in cleanroom 2:
In RCA bench:
|
In plastic beaker with magnetic stirrer in the fume hood in cleanroom 2:
|
|
| Etch rate |
|
|
|
A little higher etch rates than BHF |
| Life time of the photoresist | ~½ hour | ~½ hour | ~½ hour | ~½ hour |
| Batch size |
Plastic beaker:
PP-bath:
BHF-bath in cleanroom3:
|
Plastic beaker:
PP-bath:
RCA bench:
|
1-7 wafer of 4" at a time |
1-25 wafer of 4" at a time |
| Size of substrate |
4" wafers |
2"-6" wafers |
4" wafers |
4" wafers |
| Allowed materials |
In plastic beaker or PP-bath in the fume hood in cleanroom 2:
BHF-bath in cleanroom3:
|
In plastic beaker or PP-bath in the fume hood in cleanroom 2:
In RCA bench:
|
In plastic beaker in the fume hood in cleanroom 2:
|
|



Life time of the photoresist and blue film in BHF
Photoresist delaminates from the substrate in BHF. For standard photoresist this process starts after about or less than ½ hour but the time can vary with resist pattern. It starts by under etching the photoresist at the edges. The life time can be prolonged a little to ½ hour - 40 minutes if the photoresist is baked at 120oC.
Blue film also has a limited life time in BHF. Blue film is mainly used for back side protecting the wafer while etching on the front side. The life time of Blue film is also about ½ hour.