Jump to content

Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/Sinano3: Difference between revisions

From LabAdviser
Jml (talk | contribs)
Created page with "== The Sinano3.0 recipe == {| border="2" cellpadding="2" cellspacing="1" |+ '''Recipe Sinano3.0''' |- ! rowspan="6" align="center"| Recipe | Gas | BCl<sub>3</sub> 5 sccm, HB..."
 
Jmli (talk | contribs)
Line 1: Line 1:
== The Sinano3.0 recipe ==
== The Sinano3.0 recipe ==
 
<!-- revised 1/6-2015 by jmli -->
{| border="2" cellpadding="2" cellspacing="1"  
{| border="2" cellpadding="2" cellspacing="1"  
|+ '''Recipe Sinano3.0'''
|+ '''Recipe Sinano3.0'''
Line 75: Line 75:
|-  
|-  
|}
|}
== The Sinano3.0 recipe ==
== The Sinano3.0 recipe ==



Revision as of 14:12, 1 June 2015

The Sinano3.0 recipe

Recipe Sinano3.0
Recipe Gas BCl3 5 sccm, HBr 15 sccm
Pressure 2 mTorr, Strike 3 secs @ 5 mTorr
Power 900 W CP, 50 W PP
Temperature 20 degs
Hardware 100 mm Spacers
Time 150 secs
Conditions Run ID 417, 418 and 419
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask 110 nm zep etched down to 64 nm
Wafer WF_2A#4_feb06_2011



Nominal trench line width ' ' 30 60 90 120 150 Average Std. dev.
Etch rate nm/min 236 307 333 341 339 311 44
Sidewall angle degs 84 82 83 81 80 82 2
CD loss nm/edge 28 46 62 88 103 65 30
CD loss foot nm/edge 28 46 62 88 103 65 30
Bowing 21 32 35 33 36 31 6
Bottom curvature -30 -27 -18 14 16 -9 22
Zep etch rate 46

The Sinano3.0 recipe

Recipe Sinano3.0
Recipe Gas BCl3 5 sccm, HBr 15 sccm
Pressure 2 mTorr, Strike 3 secs @ 5 mTorr
Power 900 W CP, 50 W PP
Temperature 20 degs
Hardware 100 mm Spacers
Time 150 secs
Conditions Run ID 417, 418 and 419
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask 110 nm zep etched down to 64 nm
Wafer WF_2A#4_feb06_2011



Nominal trench line width ' ' 30 60 90 120 150 Average Std. dev.
Etch rate nm/min 236 307 333 341 339 311 44
Sidewall angle degs 84 82 83 81 80 82 2
CD loss nm/edge 28 46 62 88 103 65 30
CD loss foot nm/edge 28 46 62 88 103 65 30
Bowing 21 32 35 33 36 31 6
Bottom curvature -30 -27 -18 14 16 -9 22
Zep etch rate 46