Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300/IBE magnetic stack etch: Difference between revisions
No edit summary |
|||
Line 60: | Line 60: | ||
===Design of Experiment results=== | ===Design of Experiment results=== | ||
[[image:IBE magnetic DoE etch rate.jpg |600x300px|thumb|center|The etch rate did not show any dependency on incident angle. The shown results are fitted to the DoE data and may not give an accurate measure of etch rate.]] | {| border="1" cellspacing="1" cellpadding="2" | ||
[[image:IBE magnetic DoE Corner Angle.jpg|300x300px|thumb|center|The corner angle for the etch samples showed a dependency on all parameters. The general trends can be found from the plot, however for etch structures the resultant angle may differ.]] | |[[image:IBE magnetic DoE etch rate.jpg |600x300px|thumb|center|The etch rate did not show any dependency on incident angle. The shown results are fitted to the DoE data and may not give an accurate measure of etch rate.]] | ||
|[[image:IBE magnetic DoE Corner Angle.jpg|300x300px|thumb|center|The corner angle for the etch samples showed a dependency on all parameters. The general trends can be found from the plot, however for etch structures the resultant angle may differ.]] | |||
|} | |||
===Conclusions=== | ===Conclusions=== |
Revision as of 16:36, 15 November 2012
Results of Design of Experiments optimization of magnetic stack etching (Kristian Hagsted Rasmussen spring 2011)
Process parameters
To find the optimal parameters, Design of Experiments was applied with the intervals shown on the figure below. The final optimized recipe is listed in the table.
Parameter | Ti etch acceptance | |
---|---|---|
Neutalizer current [mA] | 450 | |
RF Power [W] | 800 | |
Beam current [mA] | 400 | |
Beam voltage [V] | 500 | |
Beam accelerator voltage | 500 | |
Ar flow to neutralizer [sccm] | 5.0 | |
Ar flow to beam [sccm] | 10.0 | |
Rotation speed [rpm] | 20 | |
Stage angle [degrees] | 5 | |
Helium backside cooling [Torr] | 37.5 |
Some SEM profile images of the etched stacks
For a good pattern transfer with IBE a large amount of redeposition on the resist edge has been observed. To reduce this redeposition the best option seems to use a photoresist just thick enough for the wanted etch depth. An alternative is sidewall sputtering at low incident angle. However experiments has shown poor cleaning rate and for narrow structures low angles will give rise to shadowing effects.
Endpoint detection with SIMS
End point detection is achieved by SIMS, and the etch rate is approximately 25 Nm/min. Resist stripping can be hard due to burned resist, to remedy this try to lower the current. Changing the currect will chance the sidewall angle and new studies of etch profiles will be necessary. For help, discussion and further info please contact Kristian Hagsted Rasmussen.
Design of Experiment results
Conclusions
- Etch rate around 20 nm/min with optimized recipe.
- Good feature definition after etch.
- Good end point detection by SIMS.
- Burned resist: Lower current, 300 mA can limit resist burning. Note this will affect pattern transfer.
- Hare ears due to redeposition, thinner resist can limit the size.