Jump to content

Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300/IBE magnetic stack etch: Difference between revisions

From LabAdviser
Khr (talk | contribs)
Khr (talk | contribs)
Line 45: Line 45:
[[image:IBE magnetic stack A19-13.jpg|300x300px|thumb|center|Magnetic stack of Ta/MnIr/NiFe/Ta/Tao/Ta/MnIr/NiFe/Ta. Redeposition of etched material at photo resist. Profile ~78°]]
[[image:IBE magnetic stack A19-13.jpg|300x300px|thumb|center|Magnetic stack of Ta/MnIr/NiFe/Ta/Tao/Ta/MnIr/NiFe/Ta. Redeposition of etched material at photo resist. Profile ~78°]]
!
!
[[image:IBE magnetic stack A16-13.jpg|300x300px|thumb|center|]]
[[image:IBE magnetic stack A16-13.jpg|300x300px|thumb|center|Etched magnetic stack with pool structure transfer. Chosen etch parameters result in severe footing]]
!
!
[[image:IBE magnetic stack A3-13.jpg|300x300px|thumb|center|]]
[[image:IBE magnetic stack A3-13.jpg|300x300px|thumb|center|Etched magnetic stack with pool structure transfer. Chosen etch parameters result in severe trenching]]
|}
|}

Revision as of 15:07, 27 September 2012

End point detection is achieved by SIMS, and the etch rate is approximately 25 Nm/min. Resist stripping can be hard due to burned resist, to remedy this try to lover the current; this will though chance the sidewall angle. For help, discussion and further info please contact Kristian Hagsted Rasmussen.

Results from the acceptance test in February 2011

Process parameters for the acceptance test

Parameter Ti etch acceptance
Neutalizer current [mA] 450
RF Power [W] 800
Beam current [mA] 400
Beam voltage [V] 500
Beam accelerator voltage 500
Ar flow to neutralizer [sccm] 5.0
Ar flow to beam [sccm] 10.0
Rotation speed [rpm] 20
Stage angle [degrees] 5
Helium backside cooling [Torr] 37.5

Some SEM profile images of the etched stacks

Magnetic stack of Ta/MnIr/NiFe/Ta/Tao/Ta/MnIr/NiFe/Ta. Redeposition of etched material at photo resist. Profile ~78°
Etched magnetic stack with pool structure transfer. Chosen etch parameters result in severe footing