New page: =Etch slow= This process development is going on to find an etch recipe that is so gentle that the resist masking material can be removed with acetone + ultrasound within hopefully 10min.... |
|||
| Line 2: | Line 2: | ||
This process development is going on to find an etch recipe that is so gentle that the resist masking material can be removed with acetone + ultrasound within hopefully 10min. This is important when a metal is to be etched as this cannot withstand plasma ashing (to remove reist mask) after the etch. | This process development is going on to find an etch recipe that is so gentle that the resist masking material can be removed with acetone + ultrasound within hopefully 10min. This is important when a metal is to be etched as this cannot withstand plasma ashing (to remove reist mask) after the etch. | ||
{| border="2" cellspacing="2" cellpadding="3" | |||
!Parameter | |||
!Si etch first try | |||
|- | |||
|Neutalizer current [mA] | |||
|450 | |||
|- | |||
|RF Power [W] | |||
|1200 | |||
|- | |||
|Beam current [mA] | |||
|400 | |||
|- | |||
|Beam voltage [V] | |||
|400 | |||
|- | |||
|Beam accelerator voltage | |||
|400 | |||
|- | |||
|Ar flow to neutralizer [sccm] | |||
|6.0 | |||
|- | |||
|Ar flow to beam [sccm] | |||
|6.0 | |||
|- | |||
|Rotation speed [rpm] | |||
|20 | |||
|- | |||
|Stage angle [degrees] | |||
|10 | |||
|- | |||
|Platen temp. [dg. Celcius] | |||
|15 | |||
|- | |||
|He cooling pressure [mTorr] | |||
|37.5 | |||
|- | |||
|Results | |||
|vvv | |||
|- | |||
|etch time [min] | |||
|40 | |||
|- | |||
|Etch rate in Si [nm/min] | |||
|19.7 | |||
|- | |||
|Total time in Acetone + ultrasound [min] | |||
|17 | |||
|- | |||
|Was the resist completely removed after acetone + ultrasound? | |||
|no | |||
|- | |||
|} | |||