Jump to content

Specific Process Knowledge/Lithography/Strip/plasmaAsher04: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Jehem (talk | contribs)
Line 18: Line 18:
The user manual, risk assessment, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=530 LabManager] - '''requires login'''
The user manual, risk assessment, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=530 LabManager] - '''requires login'''


==Process information==
'''Typical stripping parameters'''<br>
'''Typical stripping parameters'''<br>
Tested with 1.5 µm AZ 5214E on 100 mm silicon substrate.
Tested with 1.5 µm AZ 5214E on 100 mm silicon substrate.
Line 28: Line 29:
<br clear="all" />
<br clear="all" />


===Process development notes===
==Process development sections==
[[Specific Process Knowledge/Lithography/Strip/plasmaAsher04_processDevelopment|Information about process development for plasma asher 04 and plasma asher 05 can be found here.]]
*[[Specific Process Knowledge/Lithography/Strip/plasmaAsher04_processDevelopment|Stripping with plasma asher 04 and plasma asher 05]]
*[[Specific Process Knowledge/Lithography/Descum/plasmaAsher04|Descum using plasma asher 04 and plasma asher 05]]

Revision as of 09:34, 25 June 2026

Plasma Asher 4

Plasma asher 4 in cleanroom E-5.

Product name: PVA Tepla Gigabatch 380M
Year of purchase: 2024

The Plasma Asher 4 can be used for the following processes:

  • Photoresist stripping
  • Descumming
  • Surface cleaning
  • Removal of organic passivation layers and masks


Plasma asher 4 has the following material restrictions:

  • No metals allowed
  • No metal oxides allowed
  • No III-V materials allowed

The user manual, risk assessment, and contact information can be found in LabManager - requires login

Process information

Typical stripping parameters
Tested with 1.5 µm AZ 5214E on 100 mm silicon substrate.

  • O2: 100 sccm
  • N2: 100 sccm
  • Pressure (DSC): 1.3 mbar
  • Power: 1000 W
  • Time (single wafer): 20-30 minutes
  • Time (full boat): 90 minutes