Etching of Gold is done wet at Danchip making your own set up in a beaker in the fumehood. We have two different solutions:
Etching of Gold is done wet at Danchip making your own set up in a beaker in the fumehood. We have two different solutions:


# Iodine etch: KI:I<math>_2</math>:H<math>_2</math>O - 100g:25g:500ml - standard at Danchip. Can be used with AZ resist as mask.
# Iodine etch: KI:I<sub>2</sub>:H<sub>2</sub>O - 100g:25g:500ml - standard at Danchip. Can be used with AZ resist as mask.
# Aqua Regia (Kongevand): HNO<math>_3</math>:HCl - 1:3 - A very strong acid witch will etch most metals and are therefore used when you wish to remove all the gold from your wafer. '''you have to be very carefull when you work with Aqua Regia (Kongevand) It can generate nitrous gases witch are very toxic!!'''
# Aqua Regia (Kongevand): HNO<sub>3</msub>:HCl - 1:3 - A very strong acid witch will etch most metals and are therefore used when you wish to remove all the gold from your wafer. '''you have to be very carefull when you work with Aqua Regia (Kongevand) It can generate nitrous gases witch are very toxic!!'''




Line 24: Line 24:
|-
|-
|'''Chemical solution'''
|'''Chemical solution'''
|KI:I<math>_2</math>:H<math>_2</math>O  (100g:25g:500ml)
|KI:I<sub>2</sub>:H<sub>2</sub>O  (100g:25g:500ml)
|HCl:HNO<math>_3</math>  (3:1)
|HCl:HNO<sub>3</sub>  (3:1)
|-
|-
|'''Process temperature'''
|'''Process temperature'''

Revision as of 15:33, 18 October 2012

Ething of Gold can be done either wet or dry. For wet etching please see below on this page. Dry etching can be done with IBE by sputtering with Ar ions.


Etching of Gold

Wet Gold Etch: Done in the fumehood positioned in cleanroom 2

Etching of Gold is done wet at Danchip making your own set up in a beaker in the fumehood. We have two different solutions:

  1. Iodine etch: KI:I2:H2O - 100g:25g:500ml - standard at Danchip. Can be used with AZ resist as mask.
  2. Aqua Regia (Kongevand): HNO3</msub>:HCl - 1:3 - A very strong acid witch will etch most metals and are therefore used when you wish to remove all the gold from your wafer. you have to be very carefull when you work with Aqua Regia (Kongevand) It can generate nitrous gases witch are very toxic!!


Comparing the two solutions

Iodine based gold etch Aqua Regia (Kongevand)
General description

Etch of pure Gold with or without photoresist mask.

Etch of pure Gold (as stripper).

Chemical solution KI:I2:H2O (100g:25g:500ml) HCl:HNO3 (3:1)
Process temperature 20 oC 20 oC
Possible masking materials

Photoresist (1.5 µm AZ5214E)

Unmasked - used as a stripper

Etch rate

~100 nm/min

~(??) nm/min - fast etch

Batch size

1-5 4" wafers at a time

1-5 4" wafer at a time

Size of substrate

2-6" wafers

2-6" wafers