HSQ Dose Test


= Resist info =
= Resist info =
Line 11: Line 12:
** Optical and SEM images and analysis   
** Optical and SEM images and analysis   


== Results ==
= Results =
Below is overview optical images of the developed pattern:
Below is overview optical images of the developed pattern:
[[File:Dose test optical.png|frameless|625x625px|dose test optical images|left]]
[[File:Dose test optical.png|frameless|625x625px|dose test optical images|left]]

Revision as of 10:21, 10 September 2025

This page is currently under construction.

HSQ Dose Test

Resist info

  • we used a 10 % HSQ resist for a dose test. The resist info sheet could be found her.
  • spinning: in labspin 3000rpm for 40s with 2s ramp (1500 acceleration) then bake for 2 min at 165 C
  • Exposure: At 12nA ap6 (spot size 10 nm) in JEOL 9500
    • Dose test with structures (3x3)
    • Develop for 90s using manual TMAH developer
    • Optical and SEM images and analysis  

Results

Below is overview optical images of the developed pattern:

dose test optical images
dose test optical images


SEM images were recorded and analyzed from the structure shown below:


The measured and designed critical dimension are plotted vs the doses below:

dose test optical images
dose test optical images


The line width roughness (LWR) is plotted vs CD below:

dose test optical images