Specific Process Knowledge/Etch/Titanium Oxide: Difference between revisions
Appearance
| Line 34: | Line 34: | ||
|2,5 nm/min | |2,5 nm/min | ||
| | | | ||
*~ | *It has not been explored | ||
*current recipe ~8 nm/min | |||
|- | |- | ||
| Line 43: | Line 44: | ||
*Isotropic | *Isotropic | ||
| | | | ||
* | *Anisotropic | ||
|- | |- | ||
| Line 54: | Line 55: | ||
*Any size (in beaker) | *Any size (in beaker) | ||
| | | | ||
* | *Samples < 150 mm wafers on carrier | ||
*one 150 mm wafer at a time | |||
*150 mm | |||
|- | |- | ||
| Line 65: | Line 65: | ||
*Any material | *Any material | ||
| | | | ||
* | *silicon, silicon oxides and nitrides | ||
*Al, Cr, Ti (incl. oxides and nitrides) | |||
*Ta, W, Nb (incl. oxides and nitrides) | |||
|- | |- | ||
|} | |} | ||
Revision as of 15:23, 4 September 2025
Feedback to this page: click here
Etch of Titanium oxide has been test in the ICP metal etcher.
- Titanium Oxide etch using ICP metal
- Titanium Oxide etch using BHF
Comparison of Titanium Oxide (ALD) etch Methods 
| BHF | ICP Metal Etcher | |
|---|---|---|
| Generel description | Wet etch of TiO2 (ALD) | Dry etch of TiO2 |
| Etch rate range | 2,5 nm/min |
|
| Etch profile |
|
|
| Substrate size |
|
|
| Allowed materials | In beaker:
|
|