Line 32: Line 32:
! Uniformity (%)
! Uniformity (%)
| < 3.5
| < 3.5
| 3.0
| 2.7
|-
|-
! Repeatability (%)
! Repeatability (%)
Line 46: Line 46:
|+ '''Process B recipe'''
|+ '''Process B recipe'''
|-
|-
!
! colspan="2" | Step 1
! colspan="2" | Step 2
|-
|-
! width="120" | Parameter  
! width="120" | Main etch (D->E)  
! width="120" | Etch
! width="120" | Dep
! width="120" | Etch
! width="120" | Etch
! width="120" | Dep
! width="120" | Dep
|-
|-
! Gas flow (sccm)  
! Gas flow (sccm)  
| SF<sub>6</sub> 350 (1.5 s) 550
| SF<sub>6</sub> 350 O<sub>2</sub> 35
| C<sub>4</sub>F<sub>8</sub> 200
| SF<sub>6</sub> 350 (1.5 s) 550
| C<sub>4</sub>F<sub>8</sub> 200
| C<sub>4</sub>F<sub>8</sub> 200
|-
|-
! Cycle time (secs)  
! Cycle time (secs)  
| 7.0
| 4.0
| 7.0
| 7.0
| 4.0
| 4.0
|-
|-
! Pressure (mtorr)  
! Pressure (mtorr)  
| 25 (1.5 s) 90 >> 150
| 20 (1.5 s) 100
| 25
| 25 (1.5 s) 150
| 25
| 25
|-
|-
! Coil power (W)  
! Coil power (W)  
| 2800  
| 2800  
| 2000
| 2800
| 2000
| 2000
|-
|-
! Platen power (W)
! Platen power (W)
| 120 >> 140 (1.5) 45
| 130 (1.5) 40
| 0
| 0
| 140 (1.5) 45
| 0
|-
|-
! Cycles   
! Cycles   
| colspan="2" | 11 (keep fixed)
| colspan="2" | 55 (process time 10:05)
| colspan="2" | 44 (vary this)
|-
|-
! Common  
! Common  
| colspan="4" | Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers
| colspan="2" | Temperature 10 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers
|}
|}

Revision as of 10:23, 5 July 2011

Process B specifications
Parameter Specification Average result
Etch rate (µm/min) > 10 10.7
Etched depth (µm) 100 107
Scallop size (nm) < 800 685
Profile (degs) 91 +/- 1 90.7
Selectivity to AZ photoresist > 100 183
Undercut (µm) <1.5 0.89
Uniformity (%) < 3.5 2.7
Repeatability (%) <4 0.47



Process B recipe
Main etch (D->E) Etch Dep
Gas flow (sccm) SF6 350 O2 35 C4F8 200
Cycle time (secs) 7.0 4.0
Pressure (mtorr) 20 (1.5 s) 100 25
Coil power (W) 2800 2000
Platen power (W) 130 (1.5) 40 0
Cycles 55 (process time 10:05)
Common Temperature 10 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers