Specific Process Knowledge/Thin film deposition/Deposition of Germanium: Difference between revisions
Appearance
| Line 10: | Line 10: | ||
* [[/Thermal Ge evaporation Thermal Evaporator|Resistive thermal evaporation of Ge in Thermal Evaporator - Lesker]] | * [[/Thermal Ge evaporation Thermal Evaporator|Resistive thermal evaporation of Ge in Thermal Evaporator - Lesker]] | ||
Some very instrument specific deposition parameters for a now-decommissioned tool can be found here: | Some very instrument specific deposition parameters for a now-decommissioned tool can be found here: [[/Thermal Ge deposition Wordentec|Thermal deposition of Ge in Wordentec]] | ||
==Ge deposition equipment comparison== | ==Ge deposition equipment comparison== | ||
Revision as of 00:27, 8 July 2025
Feedback to this page: click here
All text by DTU Nanolab staff
Deposition of Germanium
Germanium can be deposited by thermal evaporation, e-beam evaporation, and sputtering.
Resistive Thermal evaporation
Some very instrument specific deposition parameters for a now-decommissioned tool can be found here: Thermal deposition of Ge in Wordentec
Ge deposition equipment comparison
| Thermal evaporation (Thermal Evaporator) | E-beam evaporation (E-beam evaporator (Temescal) and E-beam evaporator (10-pockets)) | Sputtering (Lesker) | Sputtering (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) | |
|---|---|---|---|---|
| General description | Thermal deposition of Ge | E-beam deposition of Ge | Sputter deposition of Ge | Sputter deposition of Ge |
| Pre-clean | none | Ar ion etch (only in E-beam evaporator Temescal) | RF Ar clean | RF Ar clean |
| Layer thickness | 10 Å to about 2000 Å | few nm to about 1 µm* | 10 Å to at least 1000 Å | 10 Å to ? |
| Deposition rate | 1 Å/s | 1 Å/s - 5 Å/s | Depends on deposition parameters | Depends on deposition parameters |
| Batch size |
Many small pieces |
|
smaller pieces |
|
| Allowed materials |
Almost any that does not degas. See the cross-contamination sheet. |
Almost any that does not degas at your intended substrate temperature. See the cross-contamination sheet. |
|
* For cumulative deposition above 600 nm please write to metal@nanolab.dtu.dk to make sure there will be enough material present in the machine.