Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano142-pxnano2: Difference between revisions

Jml (talk | contribs)
Jml (talk | contribs)
Line 71: Line 71:
image:WF_2E09a_mar23_2011-150.jpg|'''nano1.42:''' The 150 nm trenches etched 120 seconds
image:WF_2E09a_mar23_2011-150.jpg|'''nano1.42:''' The 150 nm trenches etched 120 seconds
image:WF_2E09b_mar23_2011-150.jpg|'''pxnano2:''' The 150 nm trenches etched 96 seconds
image:WF_2E09b_mar23_2011-150.jpg|'''pxnano2:''' The 150 nm trenches etched 96 seconds
{| {{table}} align="left"
| align="center" style="background:#f0f0f0;"|'''Nominal trench line width'''
| align="center" style="background:#f0f0f0;"|''''''
| align="center" style="background:#f0f0f0;"|'''30'''
| align="center" style="background:#f0f0f0;"|'''60'''
| align="center" style="background:#f0f0f0;"|'''90'''
| align="center" style="background:#f0f0f0;"|'''120'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''Average'''
| align="center" style="background:#f0f0f0;"|'''Std. dev.'''
|-
| Etch rates||nm/min||149||161||166||169||170||163||9
|-
| Sidewall angle||degs||91||91||90||90||90||90||0
|-
| CD loss||nm/edge||3||-11||-12||-34||-36||-18||17
|-
| CD loss foot||nm/edge||9||1||1||-20||-9||-4||11
|-
| Bowing||||4||4||2||6||2||4||2
|-
| Bottom curvature||||-46||-40||-37||-31||-23||-35||9
|-
| zep||nm/min||||||||||||66||
|-
|
|}
{| {{table}} align="right"
| align="center" style="background:#f0f0f0;"|'''Nominal trench line width'''
| align="center" style="background:#f0f0f0;"|''''''
| align="center" style="background:#f0f0f0;"|'''30'''
| align="center" style="background:#f0f0f0;"|'''60'''
| align="center" style="background:#f0f0f0;"|'''90'''
| align="center" style="background:#f0f0f0;"|'''120'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''Average'''
| align="center" style="background:#f0f0f0;"|'''Std. dev.'''
|-
| Etch rates||nm/min||215||232||240||243||244||235||12
|-
| Sidewall angle||degs||90||89||89||89||89||89||0
|-
| CD loss||nm/edge||1||-10||-11||-33||-33||-17||15
|-
| CD loss foot||nm/edge||6||2||1||-19||-6||-3||10
|-
| Bowing||||4||2||4||3||1||3||1
|-
| Bottom curvature||||-36||-29||-22||-19||-17||-25||8
|-
| zep||nm/min||||||||||||51||
|-
|
|}


</gallery>