Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/Sinan37: Difference between revisions
Appearance
No edit summary |
No edit summary |
||
| Line 3: | Line 3: | ||
<!--Checked for updates on 10/7-2019 - ok/jmli --> | <!--Checked for updates on 10/7-2019 - ok/jmli --> | ||
<!--Checked for updates on 24/8-2021. ok/ jmli--> | <!--Checked for updates on 24/8-2021. ok/ jmli--> | ||
<!--Checked for updates on 4/4-2025 - ok/jmli --> | |||
<!--Checked for updates on 4/4-2025 - ok/jmli --> | <!--Checked for updates on 4/4-2025 - ok/jmli --> | ||
Latest revision as of 07:37, 4 April 2025
| Nominal trench line width | ' | ' | 30 | 60 | 90 | 120 | 150 | Average | Std. dev. |
| Etch rate | nm/min | 59 | 67 | 67 | 67 | 68 | 66 | 4 | |
| Sidewall angle | degs | 84 | 86 | 84 | 86 | 86 | 85 | 1 | |
| CD loss | nm/edge | -16 | -31 | -29 | -36 | -33 | -29 | 8 | |
| CD loss foot | nm/edge | -16 | -23 | -14 | -18 | -12 | -17 | 4 | |
| Bowing | 7 | 23 | 15 | 10 | 9 | 13 | 7 | ||
| Bottom curvature | -27 | -8 | 11 | 9 | 4 | -2 | 15 | ||