Jump to content

Specific Process Knowledge/Lithography/Strip: Difference between revisions

Jehem (talk | contribs)
Jehem (talk | contribs)
Line 326: Line 326:
Please note that the ashing rate for a full boat is approximately ten times slower, than the processing time for a single substrate.
Please note that the ashing rate for a full boat is approximately ten times slower, than the processing time for a single substrate.


'''Single substrate:'''<br>
{| class="wikitable"
Test using a single 100 mm wafer in the center of the process chamber shows that 200 sccm gives the highest ashing rate.
|-
! Test setup !! Single substrate !! Full boat
|-
! scope=row| Test results
| Highest ashing rate at 200 sccm || Highest ashing rate at 200 sccm
|-
! scope=row| Wafers
| 1 || 25
|-
! scope=row| Wafer size
| 100 mm || 100 mm
|-
! scope=row| Boat position
| Center of chamber || Center of chamber
|-
! scope=row| Test wafer position
| Center of boat || Center of boat
|-
! scope=row| Total gas flow rate
| Tested parameter || Tested parameter
|-
! scope=row| Gas mix ratio
| 30% N<sub>2</sub> || 30% N<sub>2</sub>
|-
! scope=row| Chamber pressure
| 1.3 mbar || 1.3 mbar
|-
! scope=row| Power
| 1000 W || 1000 W
|-
! scope=row| Test processing time
| 2 minutes || 10 minutes
|-
! scope=row| Test average temperature
| 43°C || 47°C
|}


Total gas flow rate: tested parameter<br>
Gas mix ratio: 30% nitrogen<br>
Chamber pressure: 1.3 mbar<br>
Power: 1000 W<br>
Processing time: 2 minutes<br>
Temperature (average): 43°C
<br clear="all" />
'''Full boat:'''<br>
Test using a boat of 25 100 mm wafers in the center of the process chamber shows that 200 sccm gives the highest ashing rate.
Total gas flow rate: tested parameter<br>
Gas mix ratio: 30% nitrogen<br>
Chamber pressure: 1.3 mbar<br>
Power: 1000 W<br>
Processing time: 10 minutes<br>
Temperature (average): 43°C
<br clear="all" />