Jump to content

Specific Process Knowledge/Lithography/Strip: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Jehem (talk | contribs)
Line 272: Line 272:


==Process power for plasma asher 4 & 5==
==Process power for plasma asher 4 & 5==
<!--[[File:PA_flowRate_v1.png|320px|thumb|Ashing rate as function of total gas flow rate.|right]]-->
[[File:PA_power_v1.png|320px|thumb|Ashing rate as function of total gas flow rate.|right]]
The ashing rate is related to the power used during processing. Higher power gives higher ashing rate.
The ashing rate is related to the power used during processing. Higher power gives higher ashing rate.
<!--
 
Test using a single 100 mm wafer in the center of the process chamber shows that a power of 1000 W gives the highest ashing rate.
Test using a single 100 mm wafer in the center of the process chamber shows that a power of 1000 W gives the highest ashing rate.


Line 286: Line 286:
Temperature (average): 43°C
Temperature (average): 43°C
<br clear="all" />
<br clear="all" />
-->


==Process temperature for plasma asher 4 & 5==
==Process temperature for plasma asher 4 & 5==

Revision as of 13:57, 16 January 2025

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Strip Comparison Table

Equipment Plasma Asher 3: Descum Plasma Asher 4 Plasma Asher 5 Resist strip Lift-off
Purpose

Resist descum

Clean wafers only, no metal

All purposes

Resist strip, no metal lift off

Lift-off

Method

Plasma ashing

Plasma ashing

Plasma ashing

Solvent and ultra sound

Solvent and ultra sound

Process parameters Process gasses
  • O2 (flow unknown)
  • O2 (0-500 sccm)
  • N2 (0-500 sccm)
  • O2 (0-500 sccm)
  • N2 (0-500 sccm)
  • CF4 (0-200 sccm)
  • NA
  • NA
Max. process power

100 W (100%)

1000 W

1000 W

  • NA
  • NA
Solvent
  • NA
  • NA
  • NA
  • NMP (Remover 1165)
  • Rinse in IPA
  • NMP (Remover 1165)
  • Rinse in IPA
Substrates Batch size
  • 1 small sample
  • 1 50 mm wafer
  • 1 100 mm wafer
  • 1 small sample
  • 1 50 mm wafer
  • 1-25 100 mm wafers
  • 1-25 150 mm wafers
  • 1-25 200 mm wafers
  • 1 small sample
  • 1 50 mm wafer
  • 1-25 100 mm wafers
  • 1-25 150 mm wafers
  • 1-25 200 mm wafers
  • 1 - 25 100 mm wafers
  • 1 - 25 150 mm wafers
  • 1 - 25 100 mm wafers
  • 1 - 25 150 mm wafers
Allowed materials
  • Silicon, glass, and polymer substrates
  • Film or pattern of all but Type IV
  • No metals allowed - including metal oxides
  • No III-V materials
  • Silicon, glass, and polymer substrates
  • Film or pattern of photoresist/polymer
  • Silicon, III-V, and glass substrates
  • Film or pattern of all but Type IV
  • No metals allowed - including metal oxides
  • Silicon, glass, and polymer substrates
  • Film or pattern of photoresist/polymer
  • Silicon and glass substrates
  • Film or pattern of all but Type IV


Plasma Ashing

Photoresist stripping Descum after lithography Surface treatment of plastic, ceramic and metal Ashing of organic material
Process pressure 0.5-1.5 mbar 0.5-1.5 mbar 0.5-1.5 mbar 0.5-1.5 mbar
Process gases
  • O2 (140 sccm)
  • N2 (60 sccm)
  • O2 (70-210 sccm)
  • N2 (0-70 sccm)
O2, CF4, N2 or their mixtures O2
Process power 1000 W 150-1000 W 150-1000 W 1000 W or less for heat- sensitive materials
Process time 5-90 minutes 1-10 minutes seconds to minutes Between 0.5 and 20 hours, depending on the material
Batch size 1-25 1-25 1 wafer at a time 1 wafer at a time, use a container, e.g Petri dish



Process gas ratio for plasma asher 4 & 5

Ashing rate as function of gas mix ratio.

The ashing rate is related to the gas mix, usually expressed as percentage of nitrogen of the total amount of gas.

Test using a single 100 mm wafer in the center of the process chamber shows that 30-80% nitrogen gives the highest ashing rate.

Test parameters:
Total gas flow rate: 500 sccm
Gas mix ratio: tested parameter
DSC: not used for this test
Chamber pressure: 1.2 mbar
Power: 1000 W
Processing time: 2 minutes
Temperature (average): 43°C

Process chamber pressure for plasma asher 4 & 5

Ashing rate as function of chamber pressure.

The ashing rate is related to the chamber pressure during processing.

Test using a single 100 mm wafer in the center of the process chamber shows that a chamber pressure of 1.3 mbar gives the highest ashing rate.

Test parameters:
Total gas flow rate: 150 sccm
Gas mix ratio: 30% nitrogen
DSC: tested parameter
Chamber pressure: tested parameter
Power: 1000 W
Processing time: 2 minutes
Temperature (average): 43°C

Process gas flow rate for plasma asher 4 & 5

Ashing rate as function of total gas flow rate.

The ashing rate is related to the total gas flow rate during processing.

Test using a single 100 mm wafer in the center of the process chamber shows that a total flow rate of 200 sccm gives the highest ashing rate.

Test parameters:
Total gas flow rate: tested parameter
Gas mix ratio: 30% nitrogen
DSC: 1.3 mbar
Chamber pressure: 1.3 mbar
Power: 1000 W
Processing time: 2 minutes
Temperature (average): 43°C

Process power for plasma asher 4 & 5

Ashing rate as function of total gas flow rate.

The ashing rate is related to the power used during processing. Higher power gives higher ashing rate.

Test using a single 100 mm wafer in the center of the process chamber shows that a power of 1000 W gives the highest ashing rate.

Test parameters:
Total gas flow rate: 200 sccm
Gas mix ratio: 30% nitrogen
DSC: 1.3 mbar
Chamber pressure: 1.3 mbar
Power: tested parameter
Processing time: 2 minutes
Temperature (average): 43°C

Process temperature for plasma asher 4 & 5

Ashing rate as function of temperature.

The ashing rate is related to the temperature during processing. Higher temperature gives higher ashing rate.

Test using a single 100 mm wafer in the center of the process chamber shows that increasing processing temperature gives increasing ashing rate.

Test parameters:
Total gas flow rate: 200 sccm
Gas mix ratio: 30% nitrogen
DSC: 1.3 mbar
Chamber pressure: 1.3 mbar
Power: 1000 W
Processing time: 2 minutes
Temperature (average): tested parameter


Plasma Asher 1

Plasma asher 1 was decommissioned 2024-12-02.

Information about decommissioned tool can be found here.

Plasma Asher 2

Plasma asher 2 was decommissioned 2024-12-02.

Information about decommissioned tool can be found here.

Plasma Asher 3: Descum

Plasma Asher 3: Descum is placed A-5

The Plasma Asher 3: Descum dedicated for resist descum i.e. removal of remains resist traces after development. It has a small chamber, so you can only load a single 100 mm substrate or a few smaller pieces.

In this machine, only O2 and N2 gases are used for processes.

Typical process parameters when operating the equipment:
Process: Photoresist descum
Pressure: 0.2-0.8 mbar
Gas: O2
Power: 50-100%
Time:1 -10 minutes (depending on photoresist type and thickness)

The other materials have not been tested yet.

The user manual, user APV, and contact information can be found in LabManager - requires login

Process Information

Detailed information about descum processing on Plasma asher 3: Descum can be found here.



Plasma Asher 4

Coming soon

Plasma Asher 5

Coming soon

Resist Strip

Resist strip bench in D-3

This resist strip is only for wafers without metal and SU-8.

There are one Remover 1165 bath for stripping and one IPA bath for rinsing.

Here are the main rules for resist strip use:

  • Place the wafers in a wafer holder and put them in the first bath for 10 min, this time is depending how much resist you have on the surface.
  • After the strip rinse your wafers in the IPA bath for 2-3 min.
  • Rinse your wafers for 4-5 min. in running water after stripping.


The user manual and contact information can be found in LabManager: Resist Strip - requires login


Overview of wet bench 06 and 07

Resist Strip Lift-off
General description Wet stripping of resist Lift-off process
Chemical solution NMP Remover 1165 NMP Remover 1165
Process temperature Up to 65°C Up to 65°C
Batch size

1 - 25 wafers

1 - 25 wafers

Size of substrate
  • 100 mm wafers
  • 150 mm wafers
  • 100 mm wafers
  • 150 mm wafers
Allowed materials
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride

All metals except Type IV (Pb, Te)