Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/Slow etch: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
No edit summary
Bghe (talk | contribs)
No edit summary
Line 107: Line 107:
|+ Caption text
|+ Caption text
|-
|-
! Header text !! Header text !! Header text
! A !! Header text !! Header text
|-
|-
| Example || Example || Example
| Example || Example || Example

Revision as of 16:36, 1 July 2024

The slow etch

This work is done by Berit Herstrøm @DTU Nanolab, is nothing else is stated
The slow etch is designed to etch slow at low powers to etch thin films and to avoid overheating of samples mounted on a carrier with Capton/polyimide tape

Parameter Recipe name: Slow Etch Recipe name: Slow Etch2
Coil Power [W] 350 200
Platen Power [W] 25 50
Platen temperature [oC] 20 20
H2 flow [sccm] 15 15
CF4 flow [sccm] 30 30
Pressure [mTorr] 3 10
Typical results Slow Etch Slow Etch2
Etch of SRN ~43nm/min [measured 39-50 nm/min over a 6" wafer] 23-25 nm/min [4" on carrier]]
Etch rate of Si3N4 ~49 nm/min [4" on carrier] 24-26 nm/min [4" on carrier]
Etch rate of SiO2 ~42nm/min [41-43 nm/min over a 6" wafer] 13.7-14.7 nm/min [4" on carrier]
Etch rate in Si ñm/min 11-13 nm/min (10% load, 4" wafer on 6" carrier)
Etch rate of Mir resist ~nm/min ~17 nm/min
Tested etch time without burning the resist 3 min (6 min => resist burned) 30 min
Profile [o]

Etch Profile SEM images

Etch Uniformity maps


Test section - do not use

Caption text
A Header text Header text
Example Example Example
Example Example Example
Example Example Example