Created page with "'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thermal_Process/Furnace:_Multipurpose_annealing/Acceptance_test click here]''' ''This page is written by DTU Nanolab internal'' ==Multipurpose Anneal furnace acceptance test== The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie and DTU Nanolab. At..."
 
Pevo (talk | contribs)
Line 3: Line 3:
''This page is written by DTU Nanolab  internal''
''This page is written by DTU Nanolab  internal''


==Multipurpose Anneal furnace acceptance test==
==Resist Pyrolysis (former Multipurpose Anneal) furnace acceptance test==


The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie and DTU Nanolab.
The acceptance for the Resist Pyrolysis (former Multipurpose Anneal) furnace was performed in November 2014 by ATV Technologie and DTU Nanolab.


At the acceptance test a dry oxide layer was grown on a boat of 150 mm wafers. The oxide growth was repeated three times
At the acceptance test a dry oxide layer was grown on a boat of 150 mm wafers. The oxide growth was repeated three times