Specific Process Knowledge/Etch/ICP Metal Etcher: Difference between revisions
Appearance
| Line 7: | Line 7: | ||
{| border="2" cellspacing="1" cellpadding="3" align="center" | {| border="2" cellspacing="1" cellpadding="3" align="center" | ||
!Recipe | !Recipe Sinano# | ||
![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano3| | ![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano3|3.0]] | ||
![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano31| | ![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano31|3.1]] | ||
![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano32| | ![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano32|3.2]] | ||
![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinan33| | ![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinan33|3.3]] | ||
![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano34| | ![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano34|3.4]] | ||
![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano4| | ![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano4|4.0]] | ||
![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano35| | ![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano35|3.5]] | ||
![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano36| | ![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinano36|3.6]] | ||
![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinan33-2| | ![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinan33-2|3.3]] | ||
![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinan37| | ![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinan37|3.7]] | ||
![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinan331| | ![[Specific Process Knowledge/Etch/ICP Metal Etcher/Sinan331|3.31]] | ||
|- | |- | ||
!Cl<sub>2</sub> (sccm) | !Cl<sub>2</sub> (sccm) | ||
| Line 60: | Line 60: | ||
|- | |- | ||
! Coil power (W) | ! Coil power (W) | ||
|900 | |900 L | ||
|900 | |900 F | ||
|900 | |900 F | ||
|900 | |900 F | ||
|900 | |900 F | ||
|900 | |900 L | ||
|900 | |900 L | ||
|900 | |900 F | ||
|900 | |900 F | ||
|900 | |900 L | ||
| | | | ||
|- | |- | ||
Revision as of 15:10, 6 April 2011
Etching of nanostructures in silicon using the ICP Metal Etcher or DRIE Pegasus
| Recipe Sinano# | 3.0 | 3.1 | 3.2 | 3.3 | 3.4 | 4.0 | 3.5 | 3.6 | 3.3 | 3.7 | 3.31 | |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Cl2 (sccm) | 0 | 0 | 0 | 0 | 0 | 20 | 15 | 15 | 0 | 0 | ||
| BCl3 (sccm) | 5 | 3 | 5 | 5 | 5 | 0 | 5 | 5 | 5 | 5 | ||
| HBr (sccm) | 15 | 17 | 15 | 15 | 15 | 0 | 0 | 0 | 15 | 15 | ||
| Coil power (W) | 900 L | 900 F | 900 F | 900 F | 900 F | 900 L | 900 L | 900 F | 900 F | 900 L | ||
| Platen power (W) | 50 | 50 | 60 | 75 | 90 | 60 | 60 | 60 | 75 | 60 | ||
| Pressure (mtorr) | 2 | 2 | 2 | 2 | 2 | 2 | 5 | 10 | 2 | 10 | ||
| Temperature (oC) | 20 | 20 | 20 | 20 | 20 | 20 | 20 | 20 | 20 | 50 | ||
| Spacers (mm) | 100 | 100 | 100 | 100 | 100 | 100 | 100 | 100 | 100 | 100 | ||
| Process time (s) | 150 | 180 | 120 | 180 | 120 | 90 | 120 | 180 | 300 | 180 | ||
| Nominal line width | Etched depths (nm) | |||||||||||
| 30 nm | 198 | 231 | 147 | 214 | 163 | 227 | 185 | 170 | 295 | |||
| 60 nm | 256 | 308 | 181 | 305 | 229 | 253 | 191 | 185 | 411 | |||
| 90 nm | 259 | 335 | 195 | 342 | 255 | 251 | 222 | 253 | 566 | |||
| 120 nm | 277 | 346 | 203 | 357 | 262 | 257 | 221 | 278 | 600 | |||
| 150 nm | 269 | 341 | 205 | 369 | 265 | 262 | 225 | 280 | 647 | |||
| Nominal line width | Etch rates in trenches (nm/min) | |||||||||||
| 30 nm | 79 | 77 | 74 | 71 | 82 | 151 | 93 | 57 | 59 | |||
| 60 nm | 102 | 103 | 91 | 102 | 115 | 169 | 96 | 62 | 82 | |||
| 90 nm | 104 | 112 | 98 | 114 | 128 | 167 | 111 | 84 | 113 | |||
| 120 nm | 111 | 115 | 102 | 119 | 131 | 171 | 111 | 93 | 120 | |||
| 150 nm | 108 | 114 | 103 | 123 | 133 | 175 | 113 | 93 | 129 | |||
| zep mask parameters | ||||||||||||
| start (end) | 110 (64) | 178 (96) | 180 (110) | 180 (64) | 180 (72) | 110 (43) | 110 (34) | 180 (64) | 348 (53) | |||
| zep etch rate (nm/min) | 18 | 27 | 35 | 39 | 54 | 45 | 38 | 39 | 59 | |||