Line 530: Line 530:
*Pressure:Fully open APC valve (<2 mTorr)
*Pressure:Fully open APC valve (<2 mTorr)
*Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'  
*Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'  
|Even lower powers: 300W/25W. The profiles looks better with less roughness but also mush slower etch rate, so not as deep as the previous.
|
|
|text
<gallery caption=" C10752: SiO2 etch with Cr mask on wafer piece on Si carrier 30 min etch, EM:0/0 H2:0sccm, C4F8:6.5sccm He:100sccm O2:10sccm, Pressure:?mTorr; platen power 25W, coil power:300W" perrow="6" widths="200px" heights="150px">
<gallery caption=" C10752: SiO2 etch with Cr mask on wafer piece on Si carrier 30 min etch, EM:0/0 H2:0sccm, C4F8:6.5sccm He:100sccm O2:10sccm, Pressure:?mTorr; platen power 25W, coil power:300W" perrow="6" widths="200px" heights="150px">
File:C10752_01.jpg
File:C10752_01.jpg
Line 552: Line 552:
*Pressure:Fully open APC valve (<2 mTorr)
*Pressure:Fully open APC valve (<2 mTorr)
*Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'  
*Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'  
|Repeating with longer etch time. Low sidewall roughness, less faceting of the Cr mask. Still some trenching and bowing.
|
|
|text
<gallery caption=" C10834: SiO2 etch with Cr mask on wafer piece on Si carrier 45 min etch, EM:0/0 H2:0sccm, C4F8:6.5sccm He:100sccm O2:10sccm, Pressure:?mTorr; platen power 25W, coil power:300W" perrow="6" widths="200px" heights="150px">
<gallery caption=" C10834: SiO2 etch with Cr mask on wafer piece on Si carrier 45 min etch, EM:0/0 H2:0sccm, C4F8:6.5sccm He:100sccm O2:10sccm, Pressure:?mTorr; platen power 25W, coil power:300W" perrow="6" widths="200px" heights="150px">
File:C10834_12.jpg
File:C10834_12.jpg