At DTU Nanolab we have seven furnaces for thermal oxidation of silicon samples: Boron Drive-in + Pre-dep furnace (A1), Gate Oxide furnace (A2), Phosphorous Drive-in furnace (A3), Anneal-oxide furnace (C1), Anneal-Bond furnace (C3), Al-Anneal furnace (C3) and Multipurpose Annealing furnace. | At DTU Nanolab we have seven furnaces and one RTP (rapid thermal processor) for thermal oxidation of silicon samples: Boron Drive-in + Pre-dep furnace (A1), Gate Oxide furnace (A2), Phosphorous Drive-in furnace (A3), Anneal-oxide furnace (C1), Anneal-Bond furnace (C3), Al-Anneal furnace (C3) and Multipurpose Annealing furnace. | ||
Thermal oxidation can take place either by a dry process or by a wet process, depending on what furnace that is used for the oxidation. The film quality for a dry oxide is better than the film quality for a wet oxide with regards to density and dielectric constant. However, the oxidation rate is slow for dry oxidation. | Thermal oxidation can take place either by a dry process or by a wet process, depending on what furnace that is used for the oxidation. The film quality for a dry oxide is better than the film quality for a wet oxide with regards to density and dielectric constant. However, the oxidation rate is slow for dry oxidation. | ||
Revision as of 16:10, 8 January 2024
Feedback to this page: click here
Unless otherwise stated, this page is written by DTU Nanolab internal
Oxidation
At DTU Nanolab we have seven furnaces and one RTP (rapid thermal processor) for thermal oxidation of silicon samples: Boron Drive-in + Pre-dep furnace (A1), Gate Oxide furnace (A2), Phosphorous Drive-in furnace (A3), Anneal-oxide furnace (C1), Anneal-Bond furnace (C3), Al-Anneal furnace (C3) and Multipurpose Annealing furnace.
Thermal oxidation can take place either by a dry process or by a wet process, depending on what furnace that is used for the oxidation. The film quality for a dry oxide is better than the film quality for a wet oxide with regards to density and dielectric constant. However, the oxidation rate is slow for dry oxidation.
- Dry oxidation is used to grow 5 nm - 300 nm of oxide in the furnaces: A1, A2, A3, C1, C3, C4 and Multipurpose Anneal furnace.
- Wet oxidation is used to grow up to 3 µm of oxide in the furnaces: A1, A3, C1 and C3.
Wafers with oxide layers thicker than >3 µm can normally not be made in the cleanroom and will have to be bought (but check the wafer shop first - there might be some on stock). It is NOT allowed to oxidize the same wafers two time to get a thicker layer than 3 µm without approval
Thermal oxidation can done at temperatures up to 1150 C (but only 1100 C in C1 furnace and 1050 C the Multipurpose Anneal furnace). At these very high temperatures, the quartz tube in the furnaces might start to deform, so therefore the oxidation times are restricted:
- Maximum allowed oxidation time at 1150 C: 8 hours
- Maximum allowed oxidation time at 1100 C: 23 hours (this will result in ~3 um wet oxide)
The standard recipes, quality control limits and results for the Boron Drive-in + Pre-dep furnace (A1) and the Phosphorus Drive-in furnace (A3) can be found here:
- Standard recipes, QC limits and results for the Boron Drive-in + Predep furnace (A1)
- Standard recipes, QC limits and results for the Phosphorus Drive-in furnace (A3)
The wet oxidation rates for the Anneal-Bond furnace (C1) can be found here:
Standard recipes in the oxidation furnaces
The steps in the standard oxidation recipes in the A-stack furnaces (A1, A2 and A3) and the C-stack furnaces (C1, C3 and C4) can be found here:
Comparison of the oxidation furnaces
| Generel description | Dry and wet oxidation. Boron pre-deposition and boron drive-in of boron are also done in the furnace. | Dry oxidation of gate oxide and other very clean oxides. | Dry and wet oxidation. Phosphorous drive-in is also done in the furnace. | Dry and wet oxidation of 100 mm and 150 mm wafers. Oxidation of new wafers without RCA cleaning. Oxidation and annealing of wafers from the LPCVD furnaces and PECVD4. | Dry and wet oxidation and annealing of wafers from Wafer Bonder 02 and from PECVD4 and PECVD3. | Dry oxidation and annealing of almost all materials. | Rapid thermal processing: RTA (annealing), RTO (oxidation), RTN (nitridation) and RTH (hydrogenation). |
|---|---|---|---|---|---|---|---|
| Oxidation method |
|
|
|
|
|
|
|
| Annealing gas |
|
|
|
|
|
|
|
| Process temperature |
|
|
|
|
|
|
|
| Substrate and batch size |
|
|
|
|
|
|
|
| Allowed materials |
|
|
|
|
|
|
|
Oxidation curves
Color chart for oxide/nitride thickness
Generic calculator for wet/dry oxide thickness calculation
The following links give an approximate oxide time/thickness based on a general formula:
Deal-Grove parameters
By Kasper Reck-Nielsen February 2015
The following table contains linear and parabolic parameters for use in the Deal-Grove model for thermal oxidation. The parameters are obtained a least squares fit to data available in the furnace logbooks. Information on wafer orientation and doping concentration, which is not available in the logbooks, has not been included in calculating the parameters.
| Anneal Oxide | Anneal Bond | Boron Drive-in | Gate Oxide | Phosphor Drive-in | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Recipe | B [µm2/h] | B/A [µm/h] | RMSE [nm] | B [µm2/h] | B/A [µm/h] | RMSE [nm] | B [µm2/h] | B/A [µm/h] | RMSE [nm] | B [µm2/h] | B/A [µm/h] | RMSE [nm] | B [µm2/h] | B/A [µm/h] | RMSE [nm] |
| DRY900 | 0.000408 | 0.107 | Too little data | 0.0660 | 0.272 | 31 | 0.000390 | 0.154 | Too little data | 0.0028 | 0.079 | 4 (limited data) | 0.0507 | 0.884 | Too little data |
| DRY1000 | - | - | - | - | - | - | 0.465 | 0.838 | 20 | - | - | - | 0.641 | 1.45 | 41 |
| DRY1050 | 0.0111 | 0.526 | 27 | - | - | - | 0.0129 | 0.330 | 8 | 0.022 | 0.505 | 3 (limited data) | 0.0134 | 0.362 | 6 |
| DRY1100 | 0.020 | 0.930 | 10 | - | - | - | 0.0212 | 0.736 | 23 | - | - | - | 0.0313 | 0.553 | 14 |
| WET950 | - | - | - | - | - | 0.0716 | 1.25 | 12 | - | - | - | 0.110 | 1.17 | 11 | |
| WET1000 | 0.192 | 1.54 | 44 | - | - | 0.192 | 1.80 | 29 | - | - | - | 0.195 | 2.49 | 22 | |
| WET1050 | 0.487 | 0.965 | 29 | 0.477 | 0.899 | Too little data | 0.455 | 1.33 | 16 | - | - | - | 0.448 | 1.73 | 12 |
| WET1100 | 0.580 | 1.43 | 8 | - | - | - | 0.519 | 1.186 | 3 | - | - | - | 0.403 | 9.05 | 7 |
Wet Oxidation on <100>
The curves below are based on measurements in our specific furnaces and give more accurate results. We will still recommend to make minimum one test run if the thickness is very important.
- Wet oxidation
-
A1 Furnace <100>-Si Wet Oxidation
-
A3 Furnace <100>-Si Wet Oxidation
Dry Oxidation on <100> and <111> wafer
- Dry oxidation
-
Dry oxide on <100> wafer. The y-axis is in Å and the x-axis is in minutes.
-
Dry oxide on <111> wafer. The y-axis is in Å and the x-axis is in minutes.
Breakdown voltage measurements
Breakdown measurements have been done for A1 Boron Drive-in/Pre-dep furnace, A2 Gate Oxide furnace and A3 Phosphorus drive-in furnaces in November 2021. For E1 Oxidation (8") furnace, it has been done in Febuary 2022. The results can be found on this page: