Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch: Difference between revisions

From LabAdviser
Jml (talk | contribs)
No edit summary
Jml (talk | contribs)
No edit summary
Line 137: Line 137:
! Images
! Images
|[[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano10|Images]]
|[[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano10|Images]]
|[[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano10|Images]]
|[[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano11|Images]]
|[[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano10|Images]]
|[[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano12|Images]]
|[[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano10|Images]]
|[[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano13|Images]]
|-
|-
|}
|}

Revision as of 10:58, 28 March 2011

Recipe nano1.0 nano1.1 nano1.2 nano1.3
Tool Pegasus Pegasus Pegasus Pegasus
C4F8 (sccm) 52 52 52 52
SF6 (sccm) 38 38 38 38
O2 (sccm) 0 0 0 0
Coil power (W) 800 (forward) 600 (forward) 800 (forward) 600 (forward)
Platen power (W) 50 50 50 40
Pressure (mtorr) 4 4 4 4
Temperature (degs C) 10 10 -10 -10
Process time (s) 120 120 120 120
Nominal line width Etched depths (nm)
30 nm
60 nm
90 nm
120 nm
150 nm
Nominal line width Etch rates in trenches (nm/min)
30 nm
60 nm
90 nm
120 nm
150 nm
Etch rates in zep resist (nm/min)
One point on wafer
Images Images Images Images Images