*100 nm Cr mask etched in ICP metal with 500nm DUV neg resist (NUV 2300-0.5) and 65 nm barc. | *100 nm Cr mask etched in ICP metal with 500nm DUV neg resist (NUV 2300-0.5) and 65 nm barc. | ||
===Results=== | ===Results=== | ||
Temporary conclusions on how the process parameters affect the results in this study | '''Temporary conclusions on how the process parameters affect the results in this study:''' | ||
*Going from full wafer to small piece on Si carrier: | *Going from full wafer to small piece on Si carrier: | ||
**Seemed to give more sidewall passivation | **Seemed to give more sidewall passivation | ||
Revision as of 12:02, 13 October 2023
Feedback to this page: click here
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
| Start parameters, variations noted in the gallery headline | Recipe name: no 10 with lower platen power |
|---|---|
| Coil Power [W] | 2500 |
| Platen Power [W] | 200 |
| Platen temperature [oC] | 20 |
| H2 flow [sccm] | 25.6 |
| C4F8 flow [sccm] | 25.6 |
| He flow [sccm] | 448.7 |
| Pressure | Fully open APC valve (8-9 mTorr) |
| Electromagnetic coils (EM) 'outer coil' / 'inner coil' | '2 A' / '30 A' (PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN) |
- 100 nm Cr mask etched in ICP metal with 500nm DUV neg resist (NUV 2300-0.5) and 65 nm barc.
Results
Temporary conclusions on how the process parameters affect the results in this study:
- Going from full wafer to small piece on Si carrier:
- Seemed to give more sidewall passivation
- Platen power: lowering the platen power gives
- more sidewall passivation
- lower etch rate
- Less trenching
- Removing the H2 gave:
- less sidewall passivation
- Adding O2 gave:
- less sidewall passivation
- Process pressure/total gasflow rate
- Reducing total gasflow rate which reduced the pressur inside the chamber gave:
- less sidewall passivation
- Reduced the CD (Critical Dimensions)
- Reducing total gasflow rate which reduced the pressur inside the chamber gave:
- Coil power: Reducing coil power
- less CD loss
- more sidewall passivation
- Increasing process time:
- less sidewall passivation
- more sidewall bow
- CD loss due to larger mask faceting
- SiO2 etch with Cr mask on full wafer 6 min etch
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, O2:5sccm
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr; platen power 150W, coil power:1200W
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.6mTorr; platen power 150W, coil power:1200W
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1200W
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W
-
pitch 800 nm
Top 461 nm
@edge 437 nm
bottom 402 nm
height 916 nm
height from edge 827 nm
Cr left 83.5 nm
selectivity 55.5 -
156 nm/min
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 100W, coil power:1200W
-
pitch 800 nm
Top 444 nm
bottom 374 nm
height 718 nm
Cr left 85 nm
selectivity 48
- SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch (PLEASE DO NOT REPEAT THIS LONG TIME), H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 100W, coil power:1200W
- SiO2 etch with Cr mask on wafer piece on Si carrier 10 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W