{| border="2" cellspacing="2" cellpadding="3"
!Parameter
|Recipe name: '''no 10 with lower platen power'''
 
|-
|Coil Power [W]
|2500
|-
|Platen Power [W]
|200
|-
|Platen temperature [<sup>o</sup>C]
|20
|-
|H2 flow [sccm]
|15
|-
|C<sub>4</sub>F<sub>8</sub> flow [sccm]
|30
|-
|He flow [sccm]
|
|-
|Pressure
|Fully open APC valve (8-9 mTorr)
|-
|}

Revision as of 14:08, 27 July 2023

SiO2 Etch using resist as masking material

Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
I have do some development of a SiO2 etch with resist as masking material. I have found this fairly good recipe. For now it is the standard SiO2 etch recipes but I might change the "Standard recipe" a a later time if I find a better one. If you need to etch deeper than 1 micrometer then I advise you to split the etch in several runs with O2 cleans in between (3min TDESC Clean) or else it seems like the the etch rate is going down over time.


SiO2 Etch using aSi as masking material

Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
I am now starting up development of SiO2 etch using aSi as masking material.
The samples I use are:

  • 6" Si afters with oxide (2µm),
  • aSi (~300nm),
  • Neg. DUV reist (~60nm barc, ~350 nm resist)
  • Reticle: Danchip/Triple-D
  • Dose 230 J/m2

First I need to make sure that the resist work for pattering the aSi layer is good. If the resist is not good the final etch will also not be good.

DUV optimization

Dose test with the doses (J/m2): 200, 210, 220, 230, 240, 250, 270, 280 The aim was to get good line for 400nm pitch/200nm lines

Testing with electromagnetic coils

Parameter Recipe name: no 10 with lower platen power
Coil Power [W] 2500
Platen Power [W] 200
Platen temperature [oC] 20
H2 flow [sccm] 15
C4F8 flow [sccm] 30
He flow [sccm]
Pressure Fully open APC valve (8-9 mTorr)