Palladium may be sputter deposited in the sputter-system (Lesker). See process results here:
Palladium may be sputter deposited in the sputter-system (Lesker). See process results here:
*[[/Pd sputtering in Sputter System (Lesker) |Pd sputtering in Sputter System (Lesker)]]
*[[/Pd sputtering in Sputter System (Lesker) |Pd sputtering in Sputter System (Lesker)]]



Revision as of 23:14, 7 July 2025

Feedback to this page: click here

Unless otherwise stated, this page is written by DTU Nanolab internal

Palladium deposition

Palladium can be deposited by e-beam evaporation or DC sputtering at DTU Nanolab.

Sputtering of Palladium

Palladium may be sputter deposited in the sputter-system (Lesker). See process results here:

Equipment comparison

In the chart below you can compare the different deposition equipment:


E-beam evaporation (Temescal) E-beam evaporation (Wordentec) Sputter deposition (Sputter-System (Lesker)) Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3))
General description E-beam deposition of Pd E-beam deposition of Pd Sputter deposition of Pd Sputter deposition of Pd
Pre-clean Ar ion source none RF Ar clean RF Ar clean
Layer thickness 10 Å - 600 nm* 10 Å - 600 nm* 10 Å - 600 nm* 10 Å - ? discuss with staff
Deposition rate 0.5 Å/s to 10Å/s 2 Å/s to 10Å/s Up to 4.3 Å/s Not yet known - discuss with staff
Batch size
  • Up to 4x6" wafers
  • Up to 3x8" wafers (ask for holder)
  • smaller wafers and pieces
  • Up to 6x6" wafers (deposition on one wafer at the time)
  • Up to 6x4" wafers (deposition on one wafer at the time)
  • smaller wafers and pieces
  • 1x4" wafer or
  • 1x6" wafer or
  • several small samples
  • Up to 10x4" or 6" wafers
  • Many smaller pieces
Allowed materials Almost any that do not degas
Comment

* If depositing more than 600 nm, please write to metal@nanolab.dtu.dk well in advance to ensure that enough material is present.