Specific Process Knowledge/Lithography/EBeamLithography/JEOLPatternPreparation: Difference between revisions
Appearance
| Line 33: | Line 33: | ||
== Alignment preparation == | == Alignment preparation == | ||
===Wafer scale and chip array alignment=== | ===Wafer scale and chip array alignment=== | ||
There is two fundamentally different approaches to pattern alignment on the JEOL 9500 system. One can either do a wafer scale layout where essentially one design covering all elements of the pattern is exposed, i.e. a 1 by 1 array as defined by the ARRAY command. Or, one can expose chips instanced into an array using the ARRAY command. In the first case the pattern can only be aligned via global alignment to a single set of alignment marks defining the wafer coordinate system. In the second case, an initial wafer alignment is made but each chip can then be individually aligned to an extra set of individual chip alignment marks | There is two fundamentally different approaches to pattern alignment on the JEOL 9500 system. One can either do a wafer scale layout where essentially one design covering all elements of the pattern is exposed, i.e. a 1 by 1 array as defined by the ARRAY command. Or, one can expose chips instanced into an array using the ARRAY command. In the first case the pattern can only be aligned via global alignment to a single set of alignment marks defining the wafer coordinate system. In the second case, an initial wafer alignment is made but each chip can then be individually aligned to an extra set of individual chip alignment marks. This is illustrated below. | ||
In the wafer scale layout, L1 is exposed with a set of global alignment marks (P & Q marks) in order to allow alignment of the next wafer scale layer, L2. Thus the placement of L2 is determined entirely by a single set of alignment marks. In the chip array design, in addition to the global alignment marks (P & Q marks) chip alignment marks for each instance of the chip design is also produced. Thus the placement of each instance of L2 is determined by a local mark very close to where the pattern of L2 is actually printed for increased alignment precision. | In the wafer scale layout, L1 is exposed with a set of global alignment marks (P & Q marks) in order to allow alignment of the next wafer scale layer, L2. Thus the placement of L2 is determined entirely by a single set of alignment marks. In the chip array design, in addition to the global alignment marks (P & Q marks) chip alignment marks for each instance of the chip design is also produced. Thus the placement of each instance of L2 is determined by a local mark very close to where the pattern of L2 is actually printed for increased alignment precision. | ||
| Line 39: | Line 39: | ||
Global alignment using P & Q marks is done using the SETWFR subprogram. The P & Q mark coordinates are defined in the substrate coordinate system (X,Y). For instance, on a 4" wafer it is typical to place the P and Q marks at (-40000,0) and (40000,0), respectively. | Global alignment using P & Q marks is done using the SETWFR subprogram. The P & Q mark coordinates are defined in the substrate coordinate system (X,Y). For instance, on a 4" wafer it is typical to place the P and Q marks at (-40000,0) and (40000,0), respectively. | ||
Chip marks are different however as illustrated in the right most part of the illustration below. Chip mark coordinates refer to the local chip coordinate system (X',Y'). For instance, if a chip design has a size of 800 x 800 µm it would be | Chip marks are different however as illustrated in the right most part of the illustration below. Chip mark coordinates refer to the local chip coordinate system (X',Y'). For instance, if a chip design has a size of 800 x 800 µm it would be convenient to place chip alignment marks at M1 = (-500,500), M2 = (500,500), M3 = (500,-500) and M4 = (-500,-500). If using more than one chip mark the order must be as specified in the illustration. The JEOL system supports 1 or 4 mark chip alignment (CHIPAL 1 or CHIPAL 4). | ||
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;" | {| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;" | ||