BARC DUV42S-6 coating sequences: | |||
*'''(1201) DCH 150mm BARC 65nm''' Dispense 3ml@1000rpm; spin-off 30s@4700rpm; softbake 60s@175°C | |||
*'''(1202) DCH 100mm BARC 65nm''' Dispense 1.6ml@1000rpm; spin-off 30s@3000rpm; softbake 60s@175°C | |||
KRF M230Y coating sequences: | |||
*'''(1301) DCH 150mm M230Y 360nm''' Dispense 3ml@1000rpm; spin-off 30s@2500rpm; softbake 90s@130°C | |||
*'''(1302) DCH 100mm M230Y 360nm''' Dispense 1ml@1000rpm; spin-off 30s@2500rpm; softbake 90s@130°C | |||
KRF M35G coating sequences: | |||
*'''(1401) DCH 150mm M35G 750nm''' Dispense 3ml@1000rpm; spin-off 60s@5000rpm; softbake 90s@130°C | |||
*'''(1402) DCH 100mm M35G 750nm''' Dispense 1ml@1000rpm; spin-off 60s@5000rpm; softbake 90s@130°C | |||
*'''(1403) DCH 150mm M35G 1000nm''' Dispense 3ml@1000rpm; spin-off 60s@2630rpm; softbake 90s@130°C | |||
*'''(1404) DCH 100mm M35G 1000nm''' Dispense 1ml@1000rpm; spin-off 60s@2630rpm; softbake 90s@130°C | |||
*'''(1405) DCH 150mm M35G 1400nm''' Dispense 3ml@1000rpm; spin-off 60s@1310rpm; softbake 90s@130°C | |||
*'''(1406) DCH 100mm M35G 1400nm''' Dispense 1ml@1000rpm; spin-off 60s@1310rpm; softbake 90s@130°C | |||