Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-2/ORE with Al2O3 mask: Difference between revisions
| Line 37: | Line 37: | ||
=== Holes === | === Holes === | ||
{| border="1" style="text-align: center; width: 650px; height: 200px" | {| border="1" style="text-align: center; width: 650px; height: 200px" | ||
|+ 1μm holes recipe from March 2022 - #288 = 120 min | |+ 1μm holes recipe from March 2022 - #288 = 120 min | ||
|- | |- | ||
|-style="background:LightGray; color:Black" | |-style="background:LightGray; color:Black" | ||
! | ! [[File:17.6 holes.png|400px|thumb|'''''17.6 μm holes profile.''''']] !! Time (s) !! Pressure !! O<sub>2</sub> flow (SCCM) !! SF<sub>6</sub> flow (SCCM) !! Platen power (W) !! Coil power (W) | ||
|- | |- | ||
| '''O-step''' || 10 || 220 mTorr || 200 || 0 || 40 || 0 | | '''O-step''' || 10 || 220 mTorr || 200 || 0 || 40 || 0 | ||
Revision as of 10:49, 19 January 2023
Feedback to this page: click here
THIS PAGE IS UNDER CONSTRUCTION
By Maria Farinha @nanolab, Jan 2023
Important! The pressure settings used below may no longer be permitted, always check with the Dry etch group.
As stated by Nguyen et al., the SF6 and O2 fluxes are only separated after 4 s during the C-step. Shorter time steps than that do not execute the function of the clearing. After testing recipes with only 2 s of clearing and with no clear step, it was understood it could be eliminated, showing more depth as well as less undercut when going for shorter cycles. From then on, not CORE but ORE recipes were applied D/E = O/RE.
Moreover, during the E-step, the MFC (mass flow controller) presented a delay to read the pressure when compared with the power, creating unwanted bias. To fight it, the E-step was divided into E1 and E2. The E1 of only 2 s is enough to stabilize the pressure, and E2 the profile is etch correctly, without the unwanted bias.

Pillars
Holes
Nanoholes
| Time (s) | Pressure (valve control) | O2 flow (SCCM) | SF6 flow (SCCM) | Platen power (W) | |
|---|---|---|---|---|---|
| O-step | |||||
| R-step | |||||
| E1-step | |||||
| E2-step |