Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-2/ORE with Al2O3 mask: Difference between revisions
| Line 13: | Line 13: | ||
<br> | <br> | ||
Moreover, during the E-step, the MFC (mass flow controller) presented a delay to read the pressure when compared with the power, creating unwanted bias. To fight it, the E-step was divided into E<sub>1</sub> and E<sub>2</sub>. The E<sub>1</sub> of only 2 s is enough to stabilize the pressure, and E<sub>2</sub> the profile is etch correctly, without the unwanted bias. | Moreover, during the E-step, the MFC (mass flow controller) presented a delay to read the pressure when compared with the power, creating unwanted bias. To fight it, the E-step was divided into E<sub>1</sub> and E<sub>2</sub>. The E<sub>1</sub> of only 2 s is enough to stabilize the pressure, and E<sub>2</sub> the profile is etch correctly, without the unwanted bias. | ||
[[File:graf bias & recipes.png| | [[File:graf bias & recipes.png|600px|center|thumb|'''''CORE process graphics and recipes: a) unwanted DC bias during the E-step; b) E-step separated into two steps, E<sub>1</sub> decreased the bias.''''']] | ||
=== Pillars === | === Pillars === | ||
| Line 41: | Line 41: | ||
|+ 1μm holes recipe from March 2022 - #288 = 120 min | |+ 1μm holes recipe from March 2022 - #288 = 120 min | ||
|- | |- | ||
|-style="background: | |-style="background:LightGray; color:Black" | ||
! !! Time (s) !! Pressure !! O<sub>2</sub> flow (SCCM) !! SF<sub>6</sub> flow (SCCM) !! Platen power (W) !! Coil power (W) | ! !! Time (s) !! Pressure !! O<sub>2</sub> flow (SCCM) !! SF<sub>6</sub> flow (SCCM) !! Platen power (W) !! Coil power (W) | ||
|- | |- | ||
| Line 60: | Line 60: | ||
|+ 200nm nanoholes recipe from March 2022 | |+ 200nm nanoholes recipe from March 2022 | ||
|- | |- | ||
|-style="background: | |-style="background:LightGray; color:Black" | ||
! !! Time (s) !! Pressure (valve control) !! O<sub>2</sub> flow (SCCM) !! SF<sub>6</sub> flow (SCCM) !! Platen power (W) | ! !! Time (s) !! Pressure (valve control) !! O<sub>2</sub> flow (SCCM) !! SF<sub>6</sub> flow (SCCM) !! Platen power (W) | ||
|- | |- | ||
Revision as of 10:48, 19 January 2023
Feedback to this page: click here
THIS PAGE IS UNDER CONSTRUCTION
By Maria Farinha @nanolab, Jan 2023
Important! The pressure settings used below may no longer be permitted, always check with the Dry etch group.
As stated by Nguyen et al., the SF6 and O2 fluxes are only separated after 4 s during the C-step. Shorter time steps than that do not execute the function of the clearing. After testing recipes with only 2 s of clearing and with no clear step, it was understood it could be eliminated, showing more depth as well as less undercut when going for shorter cycles. From then on, not CORE but ORE recipes were applied D/E = O/RE.
Moreover, during the E-step, the MFC (mass flow controller) presented a delay to read the pressure when compared with the power, creating unwanted bias. To fight it, the E-step was divided into E1 and E2. The E1 of only 2 s is enough to stabilize the pressure, and E2 the profile is etch correctly, without the unwanted bias.

Pillars
Holes

| Time (s) | Pressure | O2 flow (SCCM) | SF6 flow (SCCM) | Platen power (W) | Coil power (W) | |
|---|---|---|---|---|---|---|
| O-step | 10 | 220 mTorr | 200 | 0 | 40 | 0 |
| R-step | 10 | 100% | 0 | 40 | 40 | 0 |
| E1-step | 2 | 220 mTorr | 0 | 1200 | 0 | 0 |
| E2-step | 1-5 | 220 mTorr | 0 | 1200 | 1 | 2000 |
Nanoholes
| Time (s) | Pressure (valve control) | O2 flow (SCCM) | SF6 flow (SCCM) | Platen power (W) | |
|---|---|---|---|---|---|
| O-step | |||||
| R-step | |||||
| E1-step | |||||
| E2-step |