Exposure dose for AR-N 8200 is very dependent on Post Exposure Bake (PEB) temperature. A contrast curve for four different PEB processes were obtained by the following process parameters.
Exposure dose for AR-N 8200 is very dependent on Post Exposure Bake (PEB) temperature. A contrast curve for four different PEB processes were obtained with the following process parameters.


{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 95%"
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 95%"

Revision as of 10:25, 17 March 2022

AR-N 8200

AR-N 8200 is a negative E-beam resist from Allresist, it is also known as "Medusa 82". A product presentation from Allresist is available here AR-N8200 presentation.

Allresist also provides these processing guidelines.

Contrast curve

Exposure dose for AR-N 8200 is very dependent on Post Exposure Bake (PEB) temperature. A contrast curve for four different PEB processes were obtained with the following process parameters.

AR-N 8200 Contrast Curve, Processed by THOPE, FEB 2022
Resist Spin Coat E-beam exposure PEB Development
AR-N8200.06 AllResist LabSpin E-5, 4000 rpm, 60s, softbaked 10 min @ 150 degC 09-02-2016, JBX9500 E-2, 2nA aperture 5, doses 40-600 µC/cm2, 100 nm lines and 300 nm spaces 11-02-2016, Fumehood D-2, AR-600-546, rinsed in IPA 60s. 02-03-2016 AFM Icon, F-2, ScanAsyst in Air